Steel for wave generator cam of robot harmonic speed reducer and production method of steel
By improving the continuous casting process and adding forging processes, combining vacuum degassing and rolling processes, the problems of purity and tissue uniformity of domestic production of cam steel are solved, and steel with high purity and long life are achieved, replacing foreign imports Materials have enhanced the competitiveness of the intelligent robot industry.
Patent Information
- Application Number
- CN202410942320.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology is difficult to produce in China to meet the requirements of high purity, organizational uniformity and long life of steel for robot harmonic reducer wave generator cam, resulting in foreign companies monopolizing the market and limiting the development of the intelligent robot industry.
By improving the key parameters of the continuous casting process, reducing the oxygen content and harmful elements in the steel, increasing the forging process and optimizing the rolling process, vacuum degassing + continuous casting + forging + rolling processes are adopted to control chemical composition and non-metallic inclusions The content and size of the substance can be improved to improve the purity and tissue uniformity of the steel.
The high purity and organizational uniformity of the steel for cam of the robot harmonic reducer wave generator is achieved, which improves the market competitiveness of the product, replaces imported steel from abroad, and improves production efficiency and cost competitiveness.
Smart Images

Figure BDA0004944541240000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special steel smelting, and specifically relates to a steel for a cam of a wave generator of a harmonic reducer of a robot and a production method thereof. Background Art
[0002] A robot is a machine that relies on its own power and control capabilities to achieve various functions. It converts high power at the input end into low power at the output end through a precision reducer, allowing the robot to operate according to a pre-programmed program, replacing repetitive mechanical manual operations. The use of robots to replace manual labor has been widely recognized around the world and has gradually become a field of intelligent robots with great development prospects.
[0003] The harmonic reducer is the most sophisticated type of reducer in robots. Its components include: an elliptical cam, a flexible bearing, a flexible wheel with an outer gear ring, and a rigid wheel with an inner gear ring. The inner ring of the flexible bearing is fixed on the elliptical cam, forming the input end of the harmonic reducer, and the outer ring of the flexible bearing and the flexible wheel form the output end of the harmonic reducer. When the wave generator rotates continuously, it will cause the outer gear ring of the flexible wheel and the inner gear ring of the rigid wheel to produce staggered tooth motion, thereby realizing the motion transmission function. Due to its high precision, large transmission ratio, high transmission efficiency, small size, and light weight, the harmonic reducer is gradually developing in the direction of high-end manufacturing fields such as automobile manufacturing, precision CNC machine tools, and semiconductor production equipment.
[0004] According to different structures, wave generators can be divided into cam type, roller type, disc type and other types. Cam wave generators can make the meshing of flexible wheel and rigid wheel reach the ideal state, with stable operation, high precision and high efficiency. Moreover, since the stress distribution state in the flexible wheel is improved and the load-bearing capacity is high, it is suitable for transmissions with high transmission precision requirements. At present, robot harmonic reducers mainly use cam wave generators.
[0005] The cam wave generator is composed of a cam designed and manufactured according to the motion law of the flexible wheel deformation wave, and a flexible bearing that can work in a deformed state is mounted on the outside. The deformation shape and deformation amount of the cam directly determine the deformation shape and deformation amount of the flexible wheel, which is crucial to the working ability of the entire harmonic reducer. Therefore, the design of the cam material and performance is the main content of the cam wave generator design. During high-speed operation, the cam, as an engine for transmitting kinetic energy, will be more prone to fatigue failure in advance. The long life requirement of the robot harmonic reducer wave generator cam puts forward more stringent requirements on the cam steel. In addition to meeting the requirements of high strength and high wear resistance, it must also have high purity, high structural uniformity and long fatigue life.
[0006] At present, robot harmonic reducers have long been monopolized by foreign companies. Most robot manufacturers use imported materials to manufacture key cam components in wave generators. Domestic research and development of robot harmonic reducers is in its early stages, which seriously restricts the development of my country's intelligent robot industry.
[0007] Foreign countries use die casting process to produce steel for cam of harmonic reducer wave generator of robot. The steel produced by die casting process has the advantages of high uniformity and high density, but it is difficult to guarantee the high purity requirement of cam. In order to improve the purity of steel, foreign countries also use electroslag remelting process to produce cam bearing steel. The steel produced by this process has the advantages of small and uniform distribution of non-metallic inclusions, but it also has obvious disadvantages such as low production efficiency, low production capacity, high energy consumption and high production cost. Therefore, the market competitiveness of steel produced by electroslag remelting process is very low. With the development of vacuum degassing, continuous casting and continuous rolling technology, foreign countries have gradually adopted vacuum degassing + continuous casting + continuous rolling process to produce cam steel. This process can greatly improve production efficiency and production capacity, greatly reduce energy consumption and production cost, and vacuum degassing can also significantly reduce the oxygen content of steel, reduce the size of non-metallic inclusions, and improve the purity index. Therefore, vacuum degassing continuous casting material has more competitive advantages in the market, but compared with traditional die casting and electroslag remelting process, continuous casting + continuous rolling process is difficult to guarantee the requirements of high uniformity of organization. The quality bottleneck of steel used in the cam of the wave generator of the robot harmonic reducer has limited the application of high-end harmonic reducers in aerospace, new energy equipment and other fields. Summary of the invention
[0008] The technical problem to be solved by the present invention is to provide a steel for a robot harmonic reducer wave generator cam and a production method thereof in response to the above-mentioned prior art. On the basis of the current production of bearing steel, the key parameters of the continuous casting process are improved to further reduce the oxygen content and harmful element content in the steel, reduce the content and size of non-metallic inclusions, and improve the purity; by adding forging procedures and optimizing the rolling process to improve the uniformity of carbides and organizational uniformity, the quality requirements of the steel for the robot harmonic reducer wave generator cam are met, and the product has strong market competitiveness and can replace foreign imported steel.
[0009] The technical solution adopted by the present invention to solve the above problems is: a steel for a robot harmonic reducer wave generator cam, the chemical composition of the steel is C: 0.38-0.43%, Si: 0.15-0.35%, Mn: 0.60-0.90%, Cr: 0.90-1.20%, Ni≤0.20%, Cu≤0.20%, Mo≤0.08%, Al≤0.05%, Ca≤0.0010%, S≤0.008%, P≤0.015%, Ti≤0.0012%, O≤0.0006%, As≤0.01%, Sn≤0.01%, Sb≤0.005%, Pb≤0.0015%, and the balance is Fe and unavoidable impurities. The specific chemical element design of the present invention is as follows:
[0010] 1) Determination of S content
[0011] S mainly exists in steel in the form of MnS non-metallic inclusions. Although this type of inclusion is generally a plastic inclusion and has a much lower impact on the fatigue life of steel than brittle inclusions, MnS inclusions still have a certain destructive effect on the uniformity of the organization. MnS generally has a long strip morphology, but it can also form a block morphology with "edges and corners", which can have a serious harmful effect on fatigue life. However, steel contains a small amount of S element, which can improve the cutting performance of steel, so S is determined to be ≤0.008%.
[0012] 2) Determination of P content
[0013] P is a common harmful element in steel. It is easy to cause element segregation during continuous casting and reduce the uniformity of the structure. Too high P content in steel can significantly reduce the plasticity and toughness of the steel and increase the cold brittleness of the steel. P element honors steel and is easy to cause coarse grains, so it is determined that P≤0.015%;
[0014] 3) Determination of Ti content
[0015] During the solidification of molten steel, Ti can easily combine with N or C to form TiN or Ti(C,N) non-metallic inclusions, which are usually blocky inclusions with "angular corners". Such inclusions have high hardness and seriously affect the uniformity of the structure. During operation, they are prone to cause stress concentration at the corners, which seriously reduces the fatigue life of the bearing. Therefore, the present invention requires Ti≤0.0012%
[0016] 4) Determination of O content
[0017] Oxygen naturally enters the steel during the steelmaking process and remains in the steel at a later stage. Oxygen exists in the steel mainly in the form of non-metallic inclusions such as SiO2 and Al2O3. In particular, Al2O3 inclusions seriously affect the fatigue life of bearings. A large number of fatigue life tests have shown that reducing the oxygen content is significantly beneficial to improving the purity of steel, especially reducing the content and size of oxide brittle inclusions. Therefore, the present invention requires an oxygen content of ≤0.0006%.
[0018] 5) Determination of As, Sn, Sb, and Pb content
[0019] Trace elements such as As, Sn, Sb, and Pb are all low-melting nonferrous metals and harmful elements in steel. During the solidification of molten steel, these harmful elements are easily enriched near the grain boundaries, reducing the thermoplasticity of the steel and causing cracks on the surface of the continuous casting billet. Therefore, the content of these elements in the present invention is determined to be As≤0.01%, Sn≤0.01%, Sb≤0.005%, and Pb≤0.0015%.
[0020] The main inspection items and technical indicators of the present invention are as follows:
[0021] In order to meet the uniformity of the structure of the cam of the wave generator of the harmonic reducer of the robot, the present invention requires that the austenite grain size of the steel be inspected according to GB / T6394, and the grain size rating be ≥7.
[0022] In order to meet the requirement that the cam of the wave generator of the robot harmonic reducer has a longer fatigue life, the steel is required to have a higher purity. Therefore, the present invention puts forward strict requirements on microscopic and macroscopic non-metallic inclusions and organizational uniformity.
[0023] Microscopic non-metallic inclusions include plastic inclusions of type A and type C, and brittle inclusions of type B and type D. Plastic inclusions generally have high ductility and are not prone to fatigue cracks, so these inclusions have less damage to the fatigue life of flexible bearings; brittle inclusions generally have high hardness, which can easily cause stress concentration during the operation of flexible bearings, resulting in separation from the matrix to produce fatigue cracks, affecting the fatigue life of flexible bearings, and the larger the size of these inclusions, the greater the damage to fatigue life. The present invention requires that microscopic non-metallic inclusions be inspected according to the GB / T 10561A method, and the specific requirements for the rating of microscopic non-metallic inclusions are shown in Table 1 below.
[0024] Table 1
[0025]
[0026] Macro non-metallic inclusions can easily cause severe stress concentration during the use of the wave generator cam, greatly reducing the service life of the cam. The present invention needs to inspect the macro non-metallic inclusions according to the water immersion high-frequency flaw detection method of SEP 1927 (water immersion ultrasonic determination method for purity of forged steel bars), using 5-level sensitivity detection, and the total detection volume ≥5dm 3 , macro inclusions achieve zero defects.
[0027] Since the uniformity and density of steel structure have a relatively large impact on fatigue life, the present invention requires that the steel banded structure be tested using GB / T 13299-1991, and the ferrite banded structure is required to be ≤2.5. The present invention requires that the steel be graded using ASTM E381 for steel macrostructure, requiring C≤2.0, R≤2.0, S≤2.0, and that shrinkage cavities, cracks, subcutaneous bubbles, overburning, white spots and harmful inclusions are not allowed to appear.
[0028] Another object of the present invention is to provide a method for producing steel for a cam of a harmonic reducer wave generator of a robot, wherein the blank is smelted by vacuum degassing + continuous casting. The specific production process is molten iron pretreatment - converter or electric arc furnace smelting - LF refining - RH or VD furnace vacuum degassing - large-section continuous casting CCM large continuous casting blank - forging intermediate blank - intermediate blank rolling into material - finishing. The main production process features are as follows:
[0029] (1) Molten steel smelting: The smelting raw materials must go through KR molten iron pretreatment, converter or electric arc furnace smelting, LF refining, and RH or VD furnace vacuum degassing in sequence.
[0030] First, the molten iron must be pretreated with KR to initially reduce the content of harmful elements S and P and obtain clean molten iron. The molten iron pretreatment can also reduce the amount of slag-making agents added in subsequent smelting, shorten the smelting time, and improve production efficiency.
[0031] Secondly, primary smelting is carried out in a converter or electric arc furnace, mainly to reduce the C content, transform molten iron into molten steel, adjust the content of Si and Mn elements, further remove the content of P and S elements, add clean scrap steel, strictly control the content of residual elements in scrap steel, strictly control the content of residual harmful elements in molten steel, and control the end point C of the steelmaking process to about 0.25%. According to the end point C%, add Al iron for pre-deoxidation, so that the Al content of the refining furnace is controlled at ≤0.05%, the end point P is controlled at ≤0.020%, and the steelmaking temperature is above 1600℃. The converter or electric furnace steelmaking adopts slag plug slag blocking, slag removal after the furnace and other control technology to solve the problem of high content of harmful elements As, Sn, Pb, Sb and other harmful elements in bearing steel;
[0032] In the LF refining furnace, the content of each element is precisely controlled, and attention is paid to the selection of low Ti, low Ca alloys and high-quality refractory materials. The Ti content in the molten steel is strictly controlled to make the Ti content ≤ 0.0012wt%. In the LF process, high-performance refining synthetic slag is used, and the composition of the synthetic slag is CaO-Al2O3-SiO2 ternary slag system, and argon is used for stirring. On the one hand, it can accelerate the transfer of substances between the molten steel and the refining slag, which is beneficial to the desulfurization and deoxygenation reactions. On the other hand, argon blowing can make the Al2O3 non-metallic inclusions fully float and be removed. High-quality refractory materials are used to control the amount of MgO in the molten steel, and the LF refining time is maintained for a long time. The LF time is ≥ 1h, so that the inclusions are fully floated and removed;
[0033] After LF refining, when the molten steel is vacuum degassed in the RH or VD furnace, ensure that the furnace reaches a sufficient vacuum degree and maintains sufficient circulation processing time to further remove harmful gases and non-metallic inclusions in the molten steel and improve the purity of the molten steel. The highest vacuum degree is ≤1.5mbar, and the high vacuum time is ≥15min. After breaking the air, argon soft blowing and stirring are used, and the soft blowing time is ≥25min. On the one hand, vacuum degassing is ensured, and on the other hand, inclusions are fully floated and removed;
[0034] (2) Continuous casting: square continuous casting billets with large cross-sections are used, with specifications of 300mm×340mm and above, to ensure a large compression ratio of steel in the subsequent forging and rolling process, with a compression ratio of ≥20, thereby ensuring the density of the material; before the continuous casting process, a tundish covering agent with a thickness of ≥100mm is added to the tundish to prevent the molten steel from being oxidized before continuous casting, and protective slag is added throughout the continuous casting process for protective pouring to protect the molten steel from secondary oxidation contamination; low superheat pouring is used during the continuous casting process, and the superheat is controlled at ≤35℃, which can reduce the columnar crystal area and expand the range of the equiaxed crystal area, which can not only reduce the grain size, but also effectively reduce the component segregation of the continuous casting billet, significantly improving the uniformity of the structure of the continuous casting billet; the casting speed is 0.40-0.55min / m, and the liquid level fluctuation is stable at ≤5mm; the tundish induction heating, light pressure reduction, and electromagnetic stirring technology are used to effectively improve low-magnification defects such as central porosity and shrinkage;
[0035] (3) Rolling of intermediate billets from continuous casting: After the continuous casting billets are heated in a heating furnace with a neutral or weakly oxidizing atmosphere, they are rolled into square intermediate billets of 200mm×200mm-300mm×300mm by a primary rolling mill. The heating temperature is controlled at 1050-1200℃, and the total heating time is not less than 5 hours to ensure that the billets are fully austenitized. After the billeting is completed, the intermediate billet should be slowly cooled in a pit for not less than 60 hours, which is conducive to achieving the effect of uniform organization.
[0036] (4) The intermediate billet is rolled into finished products: The intermediate billet that meets the above-mentioned dimensions is sent to a heating furnace in a neutral or weakly oxidizing atmosphere for heating and then rolled into finished steel products. The intermediate billet must be kept warm for a long time according to its size, and the total heating time must be ≥2.5h. The high-temperature diffusion heating temperature is controlled at 1050℃-1250℃, and the high-temperature diffusion time is guaranteed to be ≥1h, so that the carbides and alloy elements are fully diffused, ensuring that the organization can meet the strict requirements of the robot harmonic reducer wave generator cam bearing for organizational uniformity. After leaving the furnace, the billet is dephosphorized by high-pressure water and then rolled into bars with specifications of φ20mm-200mm by the rolling mill, with a total compression ratio of ≥20. Ensure that the final rolling temperature is ≥900℃, and after rolling is completed, it must be taken off the line and enter the slow cooling pit for slow cooling. The temperature entering the slow cooling pit is required to be ≥450℃ to prevent coarse grains. The slow cooling time is ≥60 hours, and the temperature out of the slow cooling pit must be <200℃;
[0037] (5) Finishing: After rolling, the bars must undergo finishing processes such as straightening, chamfering, and non-destructive testing of surface quality and internal quality. They can only be finally delivered after the surface quality and internal quality testing are qualified.
[0038] Compared with the prior art, the advantages of the present invention are:
[0039] (1) The grain size of steel shall be graded according to GB / T 6394, with the grain size ≥ Grade 7.
[0040] (2) Micro inclusions are tested according to GB / T 10561A method and meet the requirements of Class A fine series ≤1.5, Class A coarse series ≤1.0, Class B fine series ≤1.0, Class B coarse series ≤0.5, Class C fine series = 0, Class C coarse series = 0, Class D fine series ≤1.0, Class D coarse series ≤0.5, and Class DS ≤1.0.
[0041] (3) Macro defects are inspected according to the SEP 1927 water immersion high frequency flaw detection method, using a 5-level sensitivity test, with a total test volume of ≥5dm 3 , macro defects reach zero defects.
[0042] (4) The microstructure shall be inspected in accordance with GB / T 13299-1991 and meet the requirement of ferrite banded microstructure ≤ Grade 2.5.
[0043] (5) The macrostructure of the steel is rated in accordance with ASTM E381, meeting the requirements of C≤2.0, R≤2.0, S≤2.0, and free from defects such as shrinkage cavities, cracks, subcutaneous bubbles, overburning, white spots, and harmful inclusions. DETAILED DESCRIPTION
[0044] The technical solution of the present invention is described in more detail in conjunction with the preferred embodiments of the present invention. However, these embodiments are only descriptions of the preferred implementation methods of the present invention and cannot impose any limitation on the scope of the present invention.
[0045] The manufacturing process of the steel for the cam of the robot harmonic reducer wave generator in the embodiment of the present invention is a specific production process flow of molten iron pretreatment - converter or electric arc furnace smelting - LF refining - RH or VD furnace vacuum degassing - large-section continuous casting CCM large continuous casting billet - forging and opening intermediate billet - intermediate billet rolling into material - finishing.
[0046] Specifically, before smelting, the molten iron must be pre-treated by KR molten iron; molten steel is smelted by converter or electric furnace, using clean scrap steel and high-quality raw and auxiliary materials, the end point C of steelmaking is controlled at about 0.25%, the end point P is controlled below ≤0.020%, and the steelmaking temperature is above 1600℃; low Ti, low Ca alloys, high-quality refractory materials and high-performance refined synthetic slag are used during LF refining; sufficient vacuum and sufficient circulation processing time are maintained during vacuum degassing; protective casting is used throughout the continuous casting process, and induction heating, light pressure reduction, and electromagnetic stirring technology are used for the tundish, low superheat casting, and superheat control. ≤35℃; forging the intermediate billet, the heating temperature is controlled at 1050-1200℃, the total heating time is not less than 5 hours, the starting rolling temperature is 1130±10℃, the final rolling temperature is controlled at 850-950℃, and the intermediate billet after rolling should be slow-cooled in the pit, and the slow-cooling time is not less than 60 hours; then, the intermediate billet is rolled into bars of target size. After rolling, the bars must be slow-cooled offline at a temperature above 450℃, the slow-cooling time is ≥60 hours, and the temperature out of the slow-cooling pit must be <200℃; after slow-cooling, the bars must be straightened, chamfered, and inspected for surface quality and internal quality, and the target bar products are obtained after passing the inspection.
[0047] The chemical compositions (wt%) of the steel used for the cam bearing of the robot harmonic reducer wave generator of each embodiment of the present invention and (for comparison) the imported materials currently used in the market are shown in Tables 2 and 3.
[0048] Table 2
[0049] C Si Mn P S Cr Cu Ni Mo Al Embodiment 1 of the present invention 0.40 0.21 0.75 0.010 0.004 1.04 0.02 0.02 0.02 0.013 Embodiment 2 of the present invention 0.41 0.20 0.76 0.011 0.002 1.03 0.03 0.02 0.01 0.011 Embodiment 3 of the present invention 0.40 0.30 0.75 0.011 0.003 1.04 0.02 0.02 0.01 0.012 Contrast steel 0.42 0.21 0.77 0.017 0.012 1.05 0.07 0.03 0.02 0.030
[0050] Table 3
[0051] As Sn Sb Pb Ca Ti O Embodiment 1 of the present invention 0.0051 0.0025 0.0013 0.0010 0.0002 0.0007 0.00046 Embodiment 2 of the present invention 0.0043 0.0024 0.0018 0.0009 0.0001 0.0008 0.00048 Embodiment 3 of the present invention 0.0041 0.0028 0.0016 0.0011 0.0002 0.007 0.00043 Contrast steel 0.0063 0.0047 0.0052 0.0014 0.0010 0.0032 0.00073
[0052] From the comparison of chemical composition, it can be seen that the contents of harmful elements such as P and S in each embodiment of the present invention are much lower than those in imported materials, wherein the P content can meet the requirement of cam bearings for P content ≤ 0.015%, and the S content is much higher than the requirement of ≤ 0.008%. The contents of As, Sn, and Sb in each embodiment are lower than those in imported steel. The control of Ti content and O content is better than that of imported steel.
[0053] Table 4 Non-metallic inclusions in the steel materials of each example
[0054] A thin A thick B thin B thick C Thin C thick D Thin D thick Ds Embodiment 1 of the present invention Φ90mm 0.5 0 0 0 0 0 0.5 0 0 Embodiment 2 of the present invention Φ90mm 0 0 0 0 0 0 0.5 0.5 0.5 Embodiment 3 of the present invention Φ90mm 0.5 0 0 0 0 0 0.5 0 0 Comparison steel Φ90mm 1.5 0.5 0.5 0.5 0 0 0.5 0.5 1.0
[0055] From the inspection results of non-metallic inclusions, due to the strict control of S content, the quantity and size control of A coarse and A fine sulfides in the present invention are far superior to the control level of foreign imported materials. Due to the strict control of oxygen content in the present invention and the low control of Al content during the smelting process, the control of B, D and DS inclusions is better than foreign imported materials. In terms of purity index, the steel of the present invention fully meets the high purity requirements of steel for the cam of the wave generator of the robot harmonic reducer.
[0056] Table 5 Water immersion high frequency flaw detection data of steel materials in various embodiments
[0057] <![CDATA[Total volume detected / dm 3 > Water immersion high frequency flaw detection results Embodiment 1 of the present invention Φ90mm 6 Zero Defects Embodiment 2 of the present invention Φ90mm 6 Zero Defects Embodiment 3 of the present invention Φ90mm 6 Zero Defects Comparison steel Φ90mm 6 The maximum length of a single defect is 5mm, star point defect
[0058] Water immersion high frequency flaw detection was carried out according to SEP 1927 method, using 5-level sensitivity detection and a total detection volume of 6dm 3 Since the smelting process adopts low S and low Al control, the vacuum degassing process is used to ensure the oxygen content, and the continuous casting billet with large cross-section size is used to ensure a large compression ratio, thereby improving the density of the organization, no macro defects are found in the embodiments of the present invention, while macro defects are found in imported materials from abroad.
[0059] Table 6 Macro data of steel materials in various examples
[0060] C R S crack Shrinkage Subcutaneous bubbles Overburn White Spot Harmful inclusions Embodiment 1 of the present invention Φ90mm 1.0 1.0 1.0 none none none none none none Embodiment 2 of the present invention Φ90mm 1.0 1.0 1.0 none none none none none none Embodiment 3 of the present invention Φ90mm 1.0 1.0 1.0 none none none none none none Comparison steel Φ90mm 1.0 1.0 1.0 none none none none none none
[0061] According to ASTM E381, the macrostructure of steel is tested, and the macrostructure index of the steel of the present invention is equivalent to that of the imported steel.
[0062] Table 7 Inspection data of carbide and austenite grain size of each example steel
[0063] Banded tissue Grain size Embodiment 1 of the present invention Φ90mm 2.5 8 Embodiment 2 of the present invention Φ90mm 2.5 8 Embodiment 3 of the present invention Φ90mm 2.5 8 Comparison steel Φ90mm 3.0 7
[0064] From the perspective of grain size, the grains of the present invention are finer and more uniform than those of imported materials due to the precise control of chemical composition.
[0065] Due to the use of two-fired material forming and high-temperature diffusion process for steel rolling, the banded structure rating of the present invention is better than that of imported materials.
[0066] In summary, the present invention adopts the process of vacuum degassing + continuous casting + forging + continuous rolling to produce the steel for the cam of the wave generator of the robot harmonic reducer. The process of molten iron pretreatment, high-quality raw and auxiliary materials, high-performance refined synthetic slag, vacuum degassing and protective pouring are adopted to effectively remove harmful non-metallic inclusions and ensure the high purity of the steel. By adopting continuous casting billets with large cross-sectional sizes, two-fire rolling processes and high-temperature diffusion processes before rolling, the structural uniformity of the steel is improved, and finally high-purity and high-structural uniformity steel is obtained, thereby replacing foreign imported materials and being more competitive in production efficiency, production cost and product quality stability.
[0067] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for producing steel for a robot harmonic reducer wave generator cam, characterized in that: The method comprises: molten iron pretreatment - converter or electric arc furnace smelting - LF refining - RH or VD furnace vacuum degassing - large-section continuous casting CCM large continuous casting billet - rolling to open intermediate billet - intermediate billet rolling into products - finishing, and the main steps are as follows: (1) Molten steel smelting: The smelting raw materials are pretreated with molten iron to reduce the content of harmful elements; primary smelting is carried out in a converter or electric furnace to transform high-quality molten iron into high-quality molten steel and further remove harmful elements; low-Ti and low-Ca alloys are selected in the LF refining furnace, the content of each element is accurately controlled, high-quality refractory materials and high-performance refined synthetic slag are used, the number and form of various inclusions in the steel are controlled, and a long LF refining time is maintained so that the inclusions can be fully floated and removed; during RH vacuum degassing, sufficient vacuum is achieved in the furnace, sufficient circulation treatment time is maintained, and the ladle soft blowing time is appropriately extended to further remove harmful gases and non-metallic inclusions in the steel grade; (2) Continuous casting: square continuous casting billets with large cross-sections are used, with specifications of 300 mm × 340 mm and above, to ensure a large compression ratio of steel in the subsequent forging and rolling process, with a compression ratio of ≥20, to ensure the density of the material; protective pouring and low superheat pouring are used throughout the continuous casting process, with the superheat controlled at ≤35°C; induction heating of the tundish, light pressure reduction, and electromagnetic stirring technology are used to effectively improve low-multiple defects; (3) Rolling the intermediate billet: After the continuous casting billet is sent to the heating furnace for heating, the heating temperature is controlled at 1050-1200°C, and the total heating time is not less than 5 hours. Then, the billet is rolled into a square intermediate billet by the primary rolling mill; (4) Rolling into finished products: The intermediate billet is sent to the heating furnace for heating again and then rolled into finished steel products. The high-temperature diffusion heating temperature is controlled at 1050℃-1250℃, the high-temperature diffusion time is guaranteed to be ≥1h, and the total heating time is ≥2.5h. The billet after leaving the furnace is dephosphorized by high-pressure water and then rolled into finished products by the rolling mill. The final rolling temperature is guaranteed to be ≥900℃. After rolling is completed, the billet is taken off the line and enters the slow cooling pit for slow cooling; (5) Finishing: After rolling, the bars go through a finishing process and are finally delivered after the surface quality and internal quality are qualified by flaw detection.
2. The method for producing steel for a robot harmonic reducer wave generator cam according to claim 1, characterized in that: In the primary smelting process of the converter or electric arc furnace, the endpoint C of the steelmaking process is controlled at about 0.25%. According to the endpoint C%, Al iron is added for pre-deoxidation, so that the Al content in the refining furnace is controlled at ≤0.05%, the endpoint P is controlled at ≤0.020%, and the steelmaking temperature is above 1600℃.
3. The method for producing steel for a robot harmonic reducer wave generator cam according to claim 1, characterized in that: In the LF refining furnace, the Ti content in the molten steel is controlled to be ≤0.0012wt%, the composition of the synthetic slag is a ternary slag system of CaO-Al2O3-SiO2, and argon gas is used for stirring, and the LF time is ≥1h.
4. The method for producing steel for a robot harmonic reducer wave generator cam according to claim 1, characterized in that: When vacuum degassing is performed in an RH or VD furnace, the maximum vacuum degree is ≤1.5mbar, the high vacuum time is ≥15min, and argon soft blowing and stirring are used after breaking the air, and the soft blowing time is ≥25min.
5. The method for producing steel for cam of harmonic reducer wave generator of robot according to claim 1, characterized in that: Before the continuous casting process, a tundish covering agent is added to the tundish with a thickness of ≥100mm; during the casting process, the pulling speed is controlled at 0.40-0.55min / m, and the liquid level fluctuation is stable at ≤5mm.
6. The method for producing steel for a robot harmonic reducer wave generator cam according to claim 1, characterized in that: During the intermediate billet rolling process, the starting rolling temperature is 1130±10℃, the final rolling temperature is controlled at 850~950℃, and the billet is slowly cooled after rolling, and the slow cooling time is not less than 60 hours.
7. The method for producing steel for a robot harmonic reducer wave generator cam according to claim 1, characterized in that: After the steel is rolled, the temperature entering the slow cooling pit is required to be ≥450℃ to prevent coarse grains. The slow cooling time is ≥60 hours, and the temperature out of the slow cooling pit must be <200℃.
8. The method for producing steel for cam of wave generator of harmonic reducer of robot according to claim 1, characterized in that: The chemical composition of the molten steel after smelting meets the following requirements: C: 0.38-0.43%, Si: 0.15-0.35%, Mn: 0.60-0.90%, Cr: 0.90-1.20%, Ni≤0.20%, Cu≤0.20%, Mo≤0.08%, Al≤0.05%, Ca≤0.0010%, S≤0.008%, P≤0.015%, Ti≤0.0012%, O≤0.0006%, As≤0.01%, Sn≤0.01%, Sb≤0.005%, Pb≤0.0015%, and the balance is Fe and unavoidable impurities.
9. The method for producing steel for a robot harmonic reducer wave generator cam according to claim 1, characterized in that: The grain size of steel is tested according to GB / T 6394, and the grain size rating is ≥7. The microscopic inclusions are tested according to GB / T 10561A method, and the non-metallic inclusions meet the requirements of Class A fine system ≤1.5; Class A coarse system ≤1.0; Class B fine system ≤1.0; Class B coarse system ≤0.5; Class C fine system = 0; Class C coarse system = 0; Class D fine system ≤1.0; Class D coarse system ≤0.5; Class Ds ≤1.
0.
10. The method for producing steel for a robot harmonic reducer wave generator cam according to claim 1, characterized in that: Macro defects are inspected according to SEP 1927 water immersion high frequency flaw detection method, using 5-level sensitivity detection, and the total detection volume is ≥5dm 3 , macro defects reach zero defects; steel adopts GB / T 13299-1991 to test the steel banded structure, ferrite banded structure ≤2.5 level, steel macrostructure ASTM E381 method, requiring C≤2.0, R≤2.0, S≤2.0, and no shrinkage holes, cracks, subcutaneous bubbles, overburning, white spots and harmful inclusions.
Citation Information
Cited By
Steel material