Method for refining high-speed steel as-cast structure

By using oxides to replace carbide-forming elements during the preparation of high-speed steel and performing high-temperature diffusion and tempering, the problems of low raw material utilization, high cost and poor material toughness are solved, and efficient refinement of high-speed steel and Red hardness is improved, suitable for industrial production.

CN119040727AActive Publication Date: 2024-11-29UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202411145677.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29
Estimated Expiration
2044-08-20

Smart Images

  • Figure CN119040727A_ABST
    Figure CN119040727A_ABST
Patent Text Reader

Abstract

The invention provides a method for refining a high-speed steel as-cast structure, and relates to the technical field of high-speed steel cast ingot preparation. The method for refining the as-cast structure of the high-speed steel comprises the steps of raw material proportioning, raw material weighing, raw material smelting, suction casting forming, annealing treatment and tempering treatment. The high-speed steel material is prepared from, by mass, 0.8%-1.3% of C, 2%-10.0% of W, 2.0%-9.0% of Mo, 4.0%-5.0% of Cr, 1%-3.0% of V, 1.5%-8.0% of Co, 0-1.5% of Si, 0.2%-0.4% of Mn, 0-1.8% of Al and the balance iron and inevitable impurity elements. Through the selection of the preparation method and the selection of adding the oxide instead of part of carbide forming elements, the high-speed steel has higher utilization rate of silicon and molybdenum oxide raw materials, the traditional preparation cost is reduced, and the heat energy consumption is small; the primary carbide of the prepared high-speed steel is subjected to multiple refinement, the toughness, hardness and red hardness of the material are improved, the subsequent machinability is high, the smelting and refining process is simple, the operation difficulty is low, the process is short, the efficiency is high, and industrial large-scale production and popularization are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-speed steel ingot preparation, in particular to a method for refining high-speed steel cast structure. Background Art

[0002] High-speed steel is a high-alloy steel containing a variety of strong carbide-forming elements such as tungsten, molybdenum, chromium, and vanadium. High-performance high-speed steel usually also contains a certain amount of cobalt, such as M42 high-speed steel. After proper heat treatment, it can obtain excellent red hardness, tempering hardness and wear resistance, and is widely used in the fields of cutting tools, molds, etc.

[0003] The wear resistance of high-speed steel mainly comes from high-hardness martensite and a large number of carbides. The more carbides there are, the more evenly they are distributed, and the finer they are, the better the wear resistance. Experiments have shown that the combination of high molybdenum and low tungsten can achieve a good match between toughness and hardness, low vanadium content is beneficial to grinding performance, and the addition of cobalt makes an important contribution to heat treatment hardness and heat resistance. However, due to the high content of alloying elements in steel, after smelting or pouring, even after forging and rolling, coarse primary carbides still exist inside, severe component segregation causes the toughness of the material to deteriorate, and cracks are easily formed along the carbide boundaries.

[0004] Tungsten and molybdenum are commonly used carbide-forming elements in high-speed steel. Because molybdenum has similar properties to tungsten and weighs about half of tungsten, many high-speed steels use a high-molybdenum-low-tungsten ratio. For high-speed steels with high molybdenum content, the primary carbide contains a large amount of M2C eutectic carbide, which is a metastable phase at high temperatures and decomposes to form M6C and MC.

[0005] my country is rich in tungsten resources (tungsten oxide), accounting for 65.5% of the world's total reserves, ranking first in the world, and molybdenum resource production (molybdenum oxide) ranks second in the world. It takes a lot of energy to reduce metal oxides to elemental metals and then convert them into molybdenum iron / tungsten iron alloys.

[0006] For example: Chinese patent CN116652128A discloses a method for refining the as-cast structure of M2 high-speed steel. Obviously, the composition selection of this high-speed steel includes high-cost trace rare earth elements, and the smelting process is relatively complicated. After the continuous casting billet is formed, high-temperature diffusion treatment is required to refine the as-cast structure. The continuous casting crystallizer needs to adopt a strong cooling + weak cooling method, and the secondary cooling is accompanied by forward and reverse roller electromagnetic stirring. The operation process is complicated and difficult.

[0007] Chinese patent CN 113355587A discloses a method for improving the as-cast structure of high-speed steel and its magnesium and rare earth microalloying and increasing solidification pressure. Obviously, the raw materials selected are metal single substance raw materials. First, part of the metal raw materials and part of the graphite are used to prepare pre-deoxidized molten steel, and then other metal raw materials and remaining graphite are added to the pre-deoxidized molten steel for alloying. Then, magnesium alloy and rare earth are added under pressure for microalloying, and the ingot obtained by casting is subjected to pressurized electroslag remelting to obtain an improved ingot structure. Obviously, this method has high requirements on the composition and pressure of the molten steel, is difficult to operate, undergoes multiple different smeltings, has a long process, is difficult to operate, has high cost, and is inefficient.

[0008] Chinese patent CN1904107A discloses a process for improving the comprehensive performance of M42 high-speed steel, which requires adjusting the contents of silicon and cobalt to 0.5-0.55% and 7.9-8.1% at the same time, and making the nitrogen content in the steel 250-880ppm, and adding a certain amount of composite deoxidizer and rare earth elements before and during steel tapping, respectively, wherein the composite deoxidizer is SiAlBaCa or a mixture composed of any two or more of four substances whose main components are Si, Al, Ba and Ca respectively; therefore, the requirements for ingredients are very strict, and the addition of composite deoxidizer and rare earth elements increases the cost, which is not conducive to industrial production and promotion. Summary of the invention

[0009] In order to solve the technical problems in the prior art such as low utilization rate of raw materials for high-speed steel, high cost, large heat energy consumption, coarse primary carbides of prepared high-speed steel, reduced toughness of materials, easy cracking, the need to add high-cost rare earth elements for refinement, complex smelting and refining process, high difficulty in operation, strict requirements on component ratio, and special control of cooling in the crystallizer before casting; the embodiment of the present invention provides a method for refining the cast structure of high-speed steel with low cost, short process and full utilization of raw materials. The technical scheme is as follows:

[0010] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0011] S1. Raw material ratio: select raw materials according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single substance raw materials; in order to eliminate the influence of impurity elements, except for the oxide used, the rest are single substance raw materials with a purity higher than 99.9wt.%;

[0012] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel to obtain weighed raw materials;

[0013] S3, raw material smelting: using a non-consumable vacuum arc furnace for smelting, 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0014] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold to form a high-speed steel button ingot;

[0015] S5, high temperature diffusion treatment: high temperature diffusion treatment is performed on the S4 high speed steel button ingot to obtain a high speed steel button ingot after high temperature diffusion;

[0016] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion is tempered multiple times to obtain high-speed steel with refined cast structure.

[0017] Optionally, the high speed steel material in S1 is calculated by element mass percentage as follows: C 0.8-1.3%, W 2-10.0%, Mo2.0-9.0%, Cr 4.0-5.0%, V 1-3.0%, Co 1.5-8.0%, Si 0-1.5%, Mn 0.2-0.4%, Al 0-1.8%, and the balance is iron and unavoidable impurity elements, wherein the total amount of W and Mo is not higher than 15%, and Si and Al are added at 0.3-0.4 times the mass of the added oxide.

[0018] Optionally, the electronic balance in S2 is a high-precision electronic balance of 0.001 g with an error of ±0.03 g.

[0019] Optionally, before weighing the raw materials in S2, ultrasonic oscillation is performed in anhydrous ethanol at a frequency of 20-40 KHz and a power of 100-450 W, and then the raw materials are dried and weighed.

[0020] Optionally, S3 needs to be vacuumed to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4 Pa or less; the weighed raw materials S2 are placed in a crucible, with silicon and molybdenum oxide placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes.

[0021] Optionally, the diameter of the water-cooled copper mold in S4 is 30 mm; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network of 10.2-21 μm, and the as-cast hardness is 53-59 HRC.

[0022] Optionally, the temperature of the high temperature diffusion treatment in S5 is 1050-1250° C., the heating rate is 8-10° C. / min, and the time is 3-5 h.

[0023] Optionally, the as-cast structure of the high-speed steel button ingot after high-temperature diffusion in S5 is a quenched austenite matrix and a eutectic ledeburite network of 12-23 μm, and the hardness is 63-68 HRC.

[0024] Optionally, the multiple tempering treatments in S6 are performed 2-4 times, the temperature is 450-580° C., the heating rate is 8-10° C. / min, and the time is 2-4 h.

[0025] Optionally, the as-cast structure of the high-speed steel with refined as-cast structure in S6 is a martensitic matrix and eutectic carbides, as well as a secondary precipitation phase of 0.5-2 μm, and the tempering hardness is 66-69 HRC. It is kept at 600° C. for 60 minutes and then air-cooled. This process is repeated 4 times continuously and the surface oxide layer is removed, and the hardness obtained is 62-67.1 HRC.

[0026] Compared with the prior art, the above technical solution has at least the following beneficial effects:

[0027] The above scheme, the present invention proposes a method for refining the cast structure of high-speed steel, which can solve the technical problems in the prior art that high-speed steel has low raw material utilization rate, high cost, large heat energy consumption, coarse primary carbide of the prepared high-speed steel, reduced material toughness, easy cracking, need to add high-cost rare earth elements for refinement, complex smelting and refining process, difficult operation, strict requirements on component ratio, and special control of cooling in the crystallizer before casting.

[0028] The present invention replaces part of the carbide-forming elements with oxides, and uses aluminum and silicon as reducing agents for reduction. The reaction products are carbide-forming elements and aluminum oxide and silicon oxide, wherein aluminum oxide and silicon oxide are removed as slag system, thereby reducing production costs, avoiding technical defects caused by excessive aluminum elements, and significantly refining the network eutectic carbide.

[0029] The addition of silicon in the present invention can refine the austenite grain size, thereby refining the network eutectic carbide. In addition to being used to reduce oxides, silicon also retains a content of 0.2-1.0%. The presence of residual silicon will promote the decomposition of M2C and can effectively refine the carbide size.

[0030] The high-temperature diffusion treatment and tempering treatment of the present invention partially dissolve the metastable phase M2C, refine the primary carbides and increase the solid solubility of the matrix, promote the precipitation of secondary carbides during tempering, thereby strengthening the material, and significantly improving the room temperature hardness and red hardness.

[0031] The as-cast structure of the high-speed steel button ingot of the present invention is an isolated discontinuous austenite matrix and a eutectic ledeburite network of 10.2-21 μm, and the as-cast hardness is 53-59 HRC. Since carbide-forming elements are added in the form of oxides, the smelting cost can be reduced by 10-20%.

[0032] The high-speed steel with refined cast structure described in the present invention has a higher secondary hardening peak value than the high-speed steel prepared by the same method, better red hardness below 600°C, and higher wear resistance; it is kept at 600°C for 60 minutes and then air-cooled, and the process is repeated 4 times continuously to remove the surface oxide layer, and then the hardness obtained is 62-67.1HRC.

[0033] In summary, compared with other traditional methods, the method of the present invention has a higher utilization rate of silicon and molybdenum oxide raw materials for high-speed steel through the selection of preparation method and the selection of replacing part of the carbide-forming elements with oxides, reduces the traditional preparation cost, and has a small heat energy consumption; the primary carbide of the prepared high-speed steel is subjected to multiple refinements, which improves the toughness, hardness and red hardness of the material, has strong subsequent machinability, simple smelting and refining process, low operation difficulty, short process flow, high efficiency, and is conducive to large-scale industrial production and promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 The SEM structure of the as-cast structure of the high-speed steel with refined as-cast structure prepared by the method for refining the as-cast structure of high-speed steel according to Example 1 of the present invention;

[0036] Figure 2 The SEM structure of the as-cast structure of the high-speed steel with refined as-cast structure prepared by the method for refining the as-cast structure of the high-speed steel in Comparative Example 1 of the present invention;

[0037] Figure 3 It is the SEM structure of the cast structure of high-speed steel with refined cast structure prepared by the method for refining the cast structure of high-speed steel in comparative example 2 of the present invention. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is described below in conjunction with the accompanying drawings.

[0039] In the embodiments of the present invention, words such as "exemplarily" and "for example" are used to indicate examples, illustrations or explanations. Any embodiment or design described as "example" in the present invention should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of the word "example" is intended to present the concept in a specific way. In addition, in the embodiments of the present invention, the meaning expressed by "and / or" can be both, or it can be either of the two.

[0040] In the embodiments of the present invention, "image" and "picture" may sometimes be used interchangeably. It should be noted that when the distinction between them is not emphasized, the meanings they intend to express are consistent.

[0041] In the embodiments of the present invention, sometimes a subscript such as W1 may be written as a non-subscript such as W1. When the difference is not emphasized, the meanings to be expressed are the same.

[0042] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0043] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0044] S1. Raw material ratio: select raw materials according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single substance raw materials; in order to eliminate the influence of impurity elements, except for the oxide used, the rest are single substance raw materials with a purity higher than 99.9wt.%;

[0045] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel to obtain weighed raw materials;

[0046] S3, raw material smelting: using a non-consumable vacuum arc furnace for smelting, 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0047] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold to form a high-speed steel button ingot;

[0048] S5, high temperature diffusion treatment: high temperature diffusion treatment is performed on the S4 high speed steel button ingot to obtain a quenched high speed steel button ingot;

[0049] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion is tempered multiple times to obtain high-speed steel with refined cast structure.

[0050] In particular, the high speed steel material of S1 is calculated by element mass percentage as follows: C 0.8-1.3%, W 2-10.0%, Mo2.0-9.0%, Cr 4.0-5.0%, V 1-3.0%, Co 1.5-8.0%, Si 0-1.5%, Mn 0.2-0.4%, Al 0-1.8%, and the balance is iron and inevitable impurity elements, of which the total amount of W and Mo is not higher than 15%, and Si and Al are added according to 0.3-0.4 times the mass of the added oxide.

[0051] In particular, the electronic balance in S2 is a high-precision 0.001g electronic balance with an error of ±0.03g.

[0052] In particular, the raw materials in S2 need to be subjected to ultrasonic oscillation in anhydrous ethanol at a frequency of 20-40KHz and a power of 100-450W before being weighed, and then weighed after drying.

[0053] In particular, S3 needs to be evacuated to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4 Pa or less; the weighed raw materials S2 are placed in a crucible, with silicon and molybdenum oxide placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes.

[0054] In particular, the diameter of the water-cooled copper mold in S4 is 30 mm; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network of 10.2-21 μm, and the as-cast hardness is 53-59 HRC.

[0055] In particular, the temperature of the high temperature diffusion treatment in S5 is 1050-1250°C, the heating rate is 8-10°C / min, and the time is 3-5h.

[0056] In particular, the as-cast structure of the high-speed steel button ingot after high-temperature diffusion in S5 is a quenched austenite matrix and a eutectic ledeburite network of 12-23 μm, with a hardness of 63-68 HRC.

[0057] In particular, the number of multiple tempering treatments in S6 is 2-4 times, the temperature is 450-580°C, the heating rate is 8-10°C / min, and the time is 2-4h.

[0058] In particular, the as-cast structure of the high-speed steel with refined as-cast structure in S6 is a martensitic matrix and eutectic carbides, as well as a secondary precipitation phase of 0.5-2μm, and the tempering hardness is 66-69HRC. After being kept at 600°C for 60 minutes and then air-cooled, the process is repeated 4 times continuously to remove the surface oxide layer, and the hardness obtained is 62-67.1HRC.

[0059] Example 1

[0060] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0061] S1. Raw material ratio: raw materials are selected according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single-substance raw materials; in order to eliminate the influence of impurity elements, except for the oxides used, the rest are single-substance raw materials with a purity higher than 99.9wt.%; the high-speed steel material of this embodiment is calculated by element mass percentage as follows: C 1.1%, W2.0%, Mo 9.0%, Cr 4.0%, V 1.0%, Co 8.0%, Si 1.0%, Mn 0.2%, Al 0.7%, and the balance is iron and unavoidable impurity elements;

[0062] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel, and replace 4% molybdenum with 5% molybdenum oxide to obtain weighed raw materials; wherein, the electronic balance is a high-precision 0.001g electronic balance with an error of ±0.03g; before weighing the raw materials, ultrasonic oscillation is required in anhydrous ethanol at a frequency of 40KHz and a power of 100W, and then weighed after drying;

[0063] S3, Raw material smelting: Use non-consumable vacuum arc furnace for smelting. Before smelting the raw materials, it is necessary to evacuate to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4 Pa or less; the weighed raw material S2 is placed in a crucible, and silicon and molybdenum oxide are placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes; then 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0064] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold with a diameter of 30 mm to obtain a high-speed steel button ingot; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network (average size 10.2μm), and the hardness in the as-cast state is 59.0HRC;

[0065] S5, high temperature diffusion treatment: The S4 high speed steel button ingot is subjected to high temperature diffusion treatment at a temperature of 1150°C, a heating rate of 8°C / min, and a time of 3h to obtain an annealed high speed steel button ingot; the as-cast structure of the high speed steel button ingot after high temperature diffusion treatment is a quenched austenite matrix and a eutectic ledeburite network (average size 12.3μm), and the hardness is 68.0HRC;

[0066] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion was tempered for multiple times, the number of tempering treatments was 3 times, the temperature was 560°C, the heating rate was 10°C / min, the time was 3h, and the high-speed steel with refined cast structure was obtained.

[0067] like Figure 1As shown, the high-speed steel with refined as-cast structure prepared in this embodiment has a martensitic matrix and eutectic carbides, as well as secondary precipitation phases (0.5-2 μm). The tempering hardness is 69.5 HRC. After being kept at 600°C for 60 minutes and then air-cooled, the process is repeated 4 times continuously and the surface oxide layer is removed, and the hardness obtained is 64.7 HRC.

[0068] Comparative Example 1

[0069] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0070] S1. Raw material ratio: raw materials are selected according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single substance raw materials; in order to eliminate the influence of impurity elements, except for the oxides used, the rest are single substance raw materials with a purity higher than 99.9wt.%; the high-speed steel material of this comparative example is calculated by element mass percentage as follows: C 1.1%, W2.0%, Mo 9.0%, Cr 4.0%, V 1.0%, Co 8.0%, Si 0.6%, Mn 0.2%, and the balance is iron and unavoidable impurity elements;

[0071] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel, and replace 4% molybdenum with 5% molybdenum oxide to obtain weighed raw materials; wherein, the electronic balance is a high-precision 0.001g electronic balance with an error of ±0.03g; before weighing the raw materials, ultrasonic oscillation is required in anhydrous ethanol at a frequency of 40KHz and a power of 100W, and then weighed after drying;

[0072] S3, Raw material smelting: Use non-consumable vacuum arc furnace for smelting. Before smelting the raw materials, it is necessary to evacuate to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4 Pa or less; the weighed raw material S2 is placed in a crucible, and silicon and molybdenum oxide are placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes; then 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0073] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold with a diameter of 30 mm to obtain a high-speed steel button ingot; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network (average size 17.8μm), and the hardness in the as-cast state is 56.2HRC;

[0074] S5, high temperature diffusion treatment: The S4 high speed steel button ingot is subjected to high temperature diffusion treatment at a temperature of 1150°C, a heating rate of 8°C / min, and a time of 3h to obtain a high speed steel button ingot after high temperature diffusion; the as-cast structure of the high speed steel button ingot after high temperature diffusion treatment is a quenched austenite matrix and a eutectic ledeburite network (20.2μm), and the hardness is 66HRC;

[0075] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion was tempered for multiple times, the number of tempering treatments was 3 times, the temperature was 560°C, the heating rate was 10°C / min, the time was 3h, and the high-speed steel with refined cast structure was obtained.

[0076] like Figure 2 As shown, the as-cast structure of the high-speed steel with refined as-cast structure prepared in this comparative example is a martensitic matrix and eutectic carbides, as well as secondary precipitation phases (0.5-2 μm). The tempering hardness is 67.5 HRC, and the surface oxide layer is removed after being kept at 600°C for 60 minutes and air-cooled, which is repeated 4 times continuously, and then the hardness obtained is 62.7 HRC.

[0077] Comparative Example 2

[0078] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0079] S1. Raw material ratio: raw materials are selected according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single substance raw materials; in order to eliminate the influence of impurity elements, except for the oxides used, the rest are single substance raw materials with a purity higher than 99.9wt.%; the high-speed steel material of this comparative example is calculated by element mass percentage as follows: C 1.1%, W2.0%, Mo 9.0%, Cr 4.0%, V 1.0%, Co 8.0%, Si 1.5%, Mn 0.2%, and the balance is iron and unavoidable impurity elements;

[0080] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel, and replace 4% molybdenum with 5% molybdenum oxide to obtain weighed raw materials; wherein, the electronic balance is a high-precision 0.001g electronic balance with an error of ±0.03g; before weighing the raw materials, ultrasonic oscillation is required in anhydrous ethanol at a frequency of 40KHz and a power of 100W, and then weighed after drying;

[0081] S3, Raw material smelting: Use non-consumable vacuum arc furnace for smelting. Before smelting the raw materials, it is necessary to evacuate to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4Pa or less; the weighed raw material S2 is placed in a crucible, and silicon and molybdenum oxide are placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes; then 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0082] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold with a diameter of 30 mm to obtain a high-speed steel button ingot; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network (average size 13.8μm), and the hardness in the cast state is 58.3HRC;

[0083] S5, high temperature diffusion treatment: The S4 high speed steel button ingot is subjected to high temperature diffusion treatment at a temperature of 1150°C, a heating rate of 8°C / min, and a time of 3h to obtain a high speed steel button ingot after high temperature diffusion; the as-cast structure of the high speed steel button ingot after high temperature diffusion treatment is a quenched austenite matrix and a eutectic ledeburite network (18.5μm), and the hardness is 67.1HRC;

[0084] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion was tempered for multiple times, the number of tempering treatments was 3 times, the temperature was 560°C, the heating rate was 10°C / min, the time was 3h, and the high-speed steel with refined cast structure was obtained.

[0085] like Figure 3 As shown, the high-speed steel with refined as-cast structure prepared in this comparative example has a martensitic matrix and eutectic carbides, as well as secondary precipitation phases (0.5-2 μm). The tempering hardness is 68.4 HRC. After being kept at 600°C for 60 minutes and then air-cooled, the process is repeated 4 times continuously and the surface oxide layer is removed, and then the hardness obtained is 63.0 HRC.

[0086] Comparing Example 1 with Comparative Examples 1 and 2, Comparative Examples 1 and 2 are standard M42 high-speed steel components, and both are reduced using a single silicon reducing agent. The silicon content of Comparative Example 1 is lower than that of Comparative Example 2, and the average size of the network eutectic carbide in the as-cast structure of Comparative Example 2 is 22.5% smaller than that of Comparative Example 1. Example 1 uses aluminum and silicon composite as reducing agents, with a total content of 1.7%, and the average size of the network eutectic carbide is smaller than that of Comparative Examples 1 and 2. The as-cast hardness and tempering of Comparative Example 2 and Example 1 are slightly higher than those of Comparative Example 1, and the as-cast hardness and tempering of Example 1 are slightly higher than those of Comparative Example 2, which is caused by fine grain strengthening.

[0087] Example 2

[0088] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0089] S1. Raw material ratio: raw materials are selected according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single-substance raw materials; in order to eliminate the influence of impurity elements, except for the oxides used, the rest are single-substance raw materials with a purity higher than 99.9wt.%; the high-speed steel material of this embodiment is calculated by element mass percentage as follows: C 1.2%, W 6.0%, Mo 5.0%, Cr 4.0%, V 2.0%, Co 1.5%, Mn 0.2%, Al 1.8%, and the balance is iron and unavoidable impurity elements;

[0090] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel, and replace 4% molybdenum with 5% molybdenum oxide to obtain weighed raw materials; wherein, the electronic balance is a high-precision 0.001g electronic balance with an error of ±0.03g; before weighing the raw materials, ultrasonic oscillation is required in anhydrous ethanol at a frequency of 20KHz and a power of 200W, and then weighed after drying;

[0091] S3, Raw material smelting: Use non-consumable vacuum arc furnace for smelting. Before smelting the raw materials, it is necessary to evacuate to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4 Pa or less; the weighed raw material S2 is placed in a crucible, and silicon and molybdenum oxide are placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes; then 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0092] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold with a diameter of 30 mm to obtain a high-speed steel button ingot; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network (average size 19.8μm), and the hardness in the as-cast state is 54.3HRC;

[0093] S5, high temperature diffusion treatment: The S4 high speed steel button ingot is subjected to high temperature diffusion treatment at a temperature of 1220°C, a heating rate of 8°C / min, and a time of 3h to obtain a high speed steel button ingot after high temperature diffusion; the as-cast structure of the high speed steel button ingot after high temperature diffusion is a quenched austenite matrix and a eutectic ledeburite network (21.9μm), and the hardness is 64HRC;

[0094] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion was tempered multiple times. The number of tempering treatments was 4 times, the temperature was 555°C, the heating rate was 10°C / min, and the time was 4h to obtain a high-speed steel with a refined cast structure.

[0095] The high-speed steel with refined as-cast structure prepared in this embodiment has a martensitic matrix and eutectic carbides, as well as secondary precipitation phases (0.5-2 μm). The tempering hardness is 68 HRC. After being kept at 600°C for 60 minutes and then air-cooled, the process is repeated 4 times continuously and the surface oxide layer is removed, and the hardness obtained is 62 HRC.

[0096] Example 3

[0097] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0098] S1. Raw material ratio: raw materials are selected according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single substance raw materials; in order to eliminate the influence of impurity elements, except for the oxides used, the rest are single substance raw materials with a purity higher than 99.9wt.%; the high-speed steel material of this embodiment is calculated by element mass percentage as follows: C 0.8%, W 6.0%, Mo 5.0%, Cr 4.0%, V 2.0%, Co 5.0%, Si 0.5%, Mn 0.2%, Al 0.8%, and the balance is iron and unavoidable impurity elements;

[0099] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel, and replace 4% molybdenum with 5% molybdenum oxide to obtain weighed raw materials; wherein, the electronic balance is a high-precision 0.001g electronic balance with an error of ±0.03g; before weighing the raw materials, ultrasonic oscillation is required in anhydrous ethanol at a frequency of 40KHz and a power of 450W, and then weighed after drying;

[0100] S3, Raw material smelting: Use non-consumable vacuum arc furnace for smelting. Before smelting the raw materials, it is necessary to evacuate to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4 Pa or less; the weighed raw material S2 is placed in a crucible, and silicon and molybdenum oxide are placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes; then 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0101] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold with a diameter of 30 mm to obtain a high-speed steel button ingot; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network (average size 18.0 μm), and the hardness in the as-cast state is 55.1 HRC;

[0102] S5, high temperature diffusion treatment: The S4 high speed steel button ingot is subjected to high temperature diffusion treatment at a temperature of 1180°C, a heating rate of 8°C / min, and a time of 5h to obtain a high speed steel button ingot after high temperature diffusion; the as-cast structure of the high speed steel button ingot after high temperature diffusion is a quenched austenite matrix and a eutectic ledeburite network (20.8μm), and the hardness is 63.8HRC;

[0103] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion was tempered multiple times. The number of tempering treatments was 4 times, the temperature was 555°C, the heating rate was 10°C / min, and the time was 4h to obtain a high-speed steel with a refined cast structure.

[0104] The high-speed steel with refined as-cast structure prepared in this embodiment has a martensitic matrix and eutectic carbides, as well as secondary precipitation phases (0.5-2 μm). The tempering hardness is 68.3 HRC. After being kept at 600°C for 60 minutes and then air-cooled, the process is repeated 4 times continuously and the surface oxide layer is removed, and the hardness obtained is 63.5 HRC.

[0105] Example 4

[0106] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0107] S1. Raw material ratio: raw materials are selected according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single substance raw materials; in order to eliminate the influence of impurity elements, except for the oxides used, the rest are single substance raw materials with a purity higher than 99.9wt.%; the high-speed steel material of this embodiment is calculated by element mass percentage as follows: C 1.0%, W 6.0%, Mo 5.0%, Cr 4.0%, V 2.0%, Si 1.2%, Mn 0.2%, and the balance is iron and unavoidable impurity elements;

[0108] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel, and replace 3.8% molybdenum with 4% molybdenum oxide to obtain weighed raw materials; wherein, the electronic balance is a high-precision 0.001g electronic balance with an error of ±0.03g; before weighing the raw materials, ultrasonic oscillation is required in anhydrous ethanol at a frequency of 20KHz and a power of 100W, and then weighed after drying;

[0109] S3, Raw material smelting: Use non-consumable vacuum arc furnace for smelting. Before smelting the raw materials, it is necessary to evacuate to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4Pa or less; the weighed raw material S2 is placed in a crucible, and silicon and molybdenum oxide are placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes; then 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0110] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold with a diameter of 30 mm to obtain a high-speed steel button ingot; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network (average size 21.0 μm), and the hardness in the as-cast state is 53.5 HRC;

[0111] S5, high temperature diffusion treatment: The S4 high speed steel button ingot is subjected to high temperature diffusion treatment at a temperature of 1240°C, a heating rate of 8°C / min, and a time of 4 hours to obtain a high speed steel button ingot after high temperature diffusion; the as-cast structure of the high speed steel button ingot after high temperature diffusion is a quenched austenite matrix and a eutectic ledeburite network (23.0μm), and the hardness is 61.0HRC;

[0112] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion was tempered for multiple times, the number of tempering treatments was 3 times, the temperature was 560°C, the heating rate was 10°C / min, the time was 4.5h, and the high-speed steel with refined cast structure was obtained.

[0113] The high-speed steel with refined as-cast structure prepared in this embodiment has a martensitic matrix and eutectic carbides, as well as secondary precipitation phases (0.5-2 μm). The tempering hardness is 68.8 HRC. After being kept at 600 degrees Celsius for 60 minutes and then air-cooled, the process is repeated 4 times continuously and the surface oxide layer is removed, and the hardness obtained is 66.8 HRC.

[0114] Example 5

[0115] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0116] S1. Raw material ratio: raw materials are selected according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single substance raw materials; in order to eliminate the influence of impurity elements, except for the oxides used, the rest are single substance raw materials with a purity higher than 99.9wt.%; the high-speed steel material of this embodiment is calculated by element mass percentage as follows: C 1.3%, W10.0%, Mo 4.0%, Cr 4.0%, V 3.0%, Mn 0.4%, Al 1.5%, and the balance is iron and unavoidable impurity elements;

[0117] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel, and replace 3.8% molybdenum with 4% molybdenum oxide to obtain weighed raw materials; wherein, the electronic balance is a high-precision 0.001g electronic balance with an error of ±0.03g; before weighing the raw materials, ultrasonic oscillation is required in anhydrous ethanol at a frequency of 20KHz and a power of 100W, and then weighed after drying;

[0118] S3, Raw material smelting: Use non-consumable vacuum arc furnace for smelting. Before smelting the raw materials, it is necessary to evacuate to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4 Pa or less; the weighed raw material S2 is placed in a crucible, and silicon and molybdenum oxide are placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes; then 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0119] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold with a diameter of 30 mm to obtain a high-speed steel button ingot; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network (average size 19.6μm), and the hardness in the as-cast state is 56.6HRC;

[0120] S5, high temperature diffusion treatment: The S4 high speed steel button ingot is subjected to high temperature diffusion treatment at a temperature of 1240°C, a heating rate of 8°C / min, and a time of 3.5h to obtain a high speed steel button ingot after high temperature diffusion; the as-cast structure of the high speed steel button ingot after high temperature diffusion is a quenched austenite matrix and a eutectic ledeburite network (20.8μm), and the hardness is 66.0HRC;

[0121] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion was tempered multiple times, the number of tempering treatments was 4 times, the temperature was 540°C, the heating rate was 10°C / min, the time was 4h, and the high-speed steel with refined cast structure was obtained.

[0122] The high-speed steel with refined as-cast structure prepared in this embodiment has a martensitic matrix and eutectic carbides, as well as secondary precipitation phases (0.5-2 μm). The tempering hardness is 68.3 HRC. After being kept at 600°C for 60 minutes and then air-cooled, the process is repeated 4 times continuously and the surface oxide layer is removed, and the hardness obtained is 67.1 HRC.

[0123] Example 6

[0124] A method for refining the as-cast structure of high-speed steel, the method for refining the as-cast structure of high-speed steel comprising the following steps:

[0125] S1. Raw material ratio: raw materials are selected according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single-substance raw materials; in order to eliminate the influence of impurity elements, except for the oxides used, the rest are single-substance raw materials with a purity higher than 99.9wt.%; the high-speed steel material of this embodiment is calculated by element mass percentage as follows: C 1.3%, W10.0%, Mo 4.0%, Cr 4.0%, V 3.0%, Mn 0.4%, Si 1.2%, and the balance is iron and unavoidable impurity elements;

[0126] S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel, and replace 4% molybdenum with 5% molybdenum oxide to obtain weighed raw materials; wherein, the electronic balance is a high-precision 0.001g electronic balance with an error of ±0.03g; before weighing the raw materials, ultrasonic oscillation is required in anhydrous ethanol at a frequency of 20KHz and a power of 100W, and then weighed after drying;

[0127] S3, Raw material smelting: Use non-consumable vacuum arc furnace for smelting. Before smelting the raw materials, it is necessary to evacuate to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4 Pa or less; the weighed raw material S2 is placed in a crucible, and silicon and molybdenum oxide are placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes; then 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt;

[0128] S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold with a diameter of 30 mm to obtain a high-speed steel button ingot; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network (average size 20.6μm), and the hardness in the as-cast state is 55.6HRC;

[0129] S5, high temperature diffusion treatment: The S4 high speed steel button ingot is subjected to high temperature diffusion treatment at a temperature of 1240°C, a heating rate of 8°C / min, and a time of 3.5h to obtain a high speed steel button ingot after high temperature diffusion; the as-cast structure of the high speed steel button ingot after high temperature diffusion is a quenched austenite matrix and a eutectic ledeburite network (21.3μm), and the hardness is 64.9HRC;

[0130] S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion was tempered multiple times, the number of tempering treatments was 4 times, the temperature was 540°C, the heating rate was 10°C / min, the time was 4h, and the high-speed steel with refined cast structure was obtained.

[0131] The high-speed steel with refined as-cast structure prepared in this embodiment has a martensitic matrix and eutectic carbides, as well as secondary precipitation phases (0.5-2 μm). The tempering hardness is 67.8 HRC. After being kept at 600 degrees Celsius for 60 minutes and then air-cooled, the process is repeated 4 times continuously and the surface oxide layer is removed, and the hardness obtained is 65.8 HRC.

[0132] The above scheme, the present invention proposes a method for refining the cast structure of high-speed steel, which can solve the technical problems in the prior art that high-speed steel has low raw material utilization rate, high cost, large heat energy consumption, coarse primary carbide of the prepared high-speed steel, reduced material toughness, easy cracking, need to add high-cost rare earth elements for refinement, complex smelting and refining process, difficult operation, strict requirements on component ratio, and special control of cooling in the crystallizer before casting.

[0133] The present invention replaces part of the carbide-forming elements with oxides, and uses aluminum and silicon as reducing agents for reduction. The reaction products are carbide-forming elements and aluminum oxide and silicon oxide, wherein aluminum oxide and silicon oxide are removed as slag system, thereby reducing production costs, avoiding technical defects caused by excessive aluminum elements, and significantly refining the network eutectic carbide.

[0134] The addition of silicon in the present invention can refine the austenite grain size, thereby refining the network eutectic carbide. In addition to being used to reduce oxides, silicon also retains a content of 0.2-1.0%. The presence of residual silicon will promote the decomposition of M2C and can effectively refine the carbide size.

[0135] The high-temperature diffusion treatment and tempering treatment of the present invention partially dissolve the metastable phase M2C, refine the primary carbides and increase the solid solubility of the matrix, promote the precipitation of secondary carbides during tempering, thereby strengthening the material, and significantly improving the room temperature hardness and red hardness.

[0136] The as-cast structure of the high-speed steel button ingot of the present invention is an isolated discontinuous austenite matrix and a eutectic ledeburite network of 10.2-21 μm, and the as-cast hardness is 53-59 HRC. Since carbide-forming elements are added in the form of oxides, the smelting cost can be reduced by 10-20%.

[0137] The high-speed steel with refined cast structure described in the present invention has a higher secondary hardening peak value than the high-speed steel prepared by the same method, better red hardness below 600°C, and higher wear resistance; it is kept at 600°C for 60 minutes and then air-cooled, and the process is repeated 4 times continuously to remove the surface oxide layer, and then the hardness obtained is 62-67.1HRC.

[0138] In summary, compared with other traditional methods, the method of the present invention has a higher utilization rate of silicon and molybdenum oxide raw materials for high-speed steel through the selection of preparation method and the selection of replacing part of the carbide-forming elements with oxides, reduces the traditional preparation cost, and has a small heat energy consumption; the primary carbide of the prepared high-speed steel is subjected to multiple refinements, which improves the toughness, hardness and red hardness of the material, has strong subsequent machinability, simple smelting and refining process, low operation difficulty, short process flow, high efficiency, and is conducive to large-scale industrial production and promotion.

[0139] It should be understood that the term "and / or" in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship, but it may also indicate an "and / or" relationship. Please refer to the context for specific understanding.

[0140] In the present invention, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, at least one of a, b, or c can mean: a, b, c, ab, ac, bc, or abc, where a, b, and c can be single or multiple.

[0141] It should be understood that in various embodiments of the present invention, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.

[0142] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for refining the as-cast structure of high-speed steel, characterized in that: The method for refining the high-speed steel cast structure comprises the following steps: S1. Raw material ratio: select raw materials according to the elements in high-speed steel to obtain selected raw materials; wherein, molybdenum oxide is used to replace part of the required molybdenum single substance raw materials; in order to eliminate the influence of impurity elements, except for the oxide used, the rest are single substance raw materials with a purity higher than 99.9wt.%; S2. Raw material weighing: Use an electronic balance to weigh and proportion the raw materials selected in S1 according to the weight ratio of each element in the high-speed steel to obtain weighed raw materials; S3, raw material smelting: using a non-consumable vacuum arc furnace for smelting, 50g of the weighed raw material S2 is placed in a crucible for raw material smelting to obtain an alloy melt; S4, suction casting: vacuum suction casting is used to directly suck the alloy melt of S3 into a water-cooled copper mold to form a high-speed steel button ingot; S5, high temperature diffusion treatment: high temperature diffusion treatment is performed on the S4 high speed steel button ingot to obtain a high speed steel button ingot after high temperature diffusion; S6. Tempering treatment: The high-speed steel button ingot after S5 high-temperature diffusion is tempered multiple times to obtain high-speed steel with refined cast structure.

2. The method for refining the as-cast structure of high-speed steel according to claim 1, characterized in that: The high speed steel materials of S1 are calculated by element mass percentage as follows: C 0.8-1.3%, W 2-10.0%, Mo 2.0-9.0%, Cr 4.0-5.0%, V 1-3.0%, Co1.5-8.0%, Si 0-1.5%, Mn 0.2-0.4%, Al 0-1.8%, and the balance is iron and unavoidable impurity elements, of which the total amount of W and Mo is not higher than 15%, and Si and Al are added at 0.3-0.4 times the mass of the added oxide.

3. The method for refining the as-cast structure of high-speed steel according to claim 1, characterized in that: The electronic balance in S2 is a high-precision 0.001g electronic balance with an error of ±0.03g.

4. The method for refining the as-cast structure of high-speed steel according to claim 1, characterized in that: Before weighing the raw materials in S2, ultrasonic vibration is required in anhydrous ethanol at a frequency of 20-40KHz and a power of 100-450W, and then weighed after drying.

5. The method for refining the as-cast structure of high-speed steel according to claim 1, characterized in that: Before smelting the raw materials, S3 needs to be vacuumed to 5×10 -3 Pa, fill with high-purity argon gas, repeat the above steps, and evacuate to 5×10 -4 Pa or less; the weighed raw materials S2 are placed in a crucible, with silicon and molybdenum oxide placed together; the raw material smelting needs to be repeated more than 8 times, each time for 2 minutes.

6. The method for refining the as-cast structure of high-speed steel according to claim 1, characterized in that: The diameter of the water-cooled copper mold in S4 is 30 mm; the as-cast structure of the high-speed steel button ingot is an isolated discontinuous austenite matrix and a eutectic ledeburite network of 10.2-21 μm, and the hardness in the as-cast state is 53-59 HRC.

7. The method for refining the as-cast structure of high-speed steel according to claim 1, characterized in that: The temperature of the high temperature diffusion treatment in S5 is 1050-1250°C, the heating rate is 8-10°C / min, and the time is 3-5h.

8. The method for refining high-speed steel cast structure according to claim 1, characterized in that: The as-cast structure of S5 high-speed steel button ingot after medium and high temperature diffusion is quenched austenite matrix and 12-23μm eutectic ledeburite network, with a hardness of 63-68HRC.

9. The method for refining the as-cast structure of high-speed steel according to claim 1, characterized in that: The number of multiple tempering treatments in S6 is 2-4 times, the temperature is 450-580°C, the heating rate is 8-10°C / min, and the time is 2-4h.

10. The method for refining the as-cast structure of high-speed steel according to claim 1, characterized in that: The as-cast structure of the high-speed steel with refined as-cast structure in S6 is a martensitic matrix and eutectic carbides, as well as a secondary precipitation phase of 0.5-2μm. The tempering hardness is 66-69HRC. After being kept at 600℃ for 60min and then air-cooled, the process is repeated 4 times continuously to remove the surface oxide layer, and the hardness obtained is 62-67.1HRC.

Citation Information

Patent Citations

  • Low-alloy high speed steel roll material and preparation method thereof

    CN101078090A

  • Method for preparing regenerated high-speed steel material through electroslag metallurgy and adding rear earth oxide

    CN102776380A

  • Electric furnace steel making process capable of simultaneously and directly alloying manganese oxide and molybdenum oxide

    CN106636540A

  • Technology for alloying-smelting semi-high-speed-steel roller steel from wolframite concentrate in medium-frequency furnace

    CN109913644A

  • Molybdenum-containing stainless steel smelting method for inhibiting volatilization and splashing of molybdenum oxide

    CN111910116A

Cited By

  • Preparation method of high-speed steel composite material

    CN120818729A

  • A method for producing a high speed steel composite

    CN120818729B