Smelting method of steel for ultrahigh-strength precision welded pipe

Through the method of blowing argon out of steel and end deoxygenation of small-platform magnesium-aluminum alloy wires throughout the process, the problem of inclusion control insulated in the smelting of steel for ultra-high strength precision welded pipes is solved, and the smelting effect with high quality and high cleanliness is achieved.

CN119040729APending Publication Date: 2024-11-29PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411278490.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove inclusions during the smelting of steel for ultra-high strength precision welded pipes, resulting in cracking. The existing deoxidation methods are inefficient and costly.

Method used

The method of final deoxygenation of steel with argon blown out of steel and small-platform magnesium-aluminum alloy wires is adopted to inhibit the absorption of nitrogen by liquid steel, generate fine and dispersed aluminum deoxygenation products, and improve the control of inclusions.

Benefits of technology

The high-quality and cleanliness and high-strength precision welded pipe steel smelting has been achieved, which significantly reduces the generation of inclusions and improves the quality and cleanliness of the finished product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a smelting method of steel for an ultrahigh-strength precision welded pipe, which comprises the following steps: S1) carrying out converter vanadium extraction and desulfurization pretreatment on vanadium-containing molten iron to obtain semi-steel; s2, the semi-steel is subjected to primary smelting in a converter, and molten steel is obtained; (S3) the molten steel is subjected to whole-course argon blowing tapping, active lime is added in a mixed flushing mode after 2 / 3 of tapping, aluminum deoxidation is not needed during tapping, alloying is conducted through a low-nitrogen carbonaceous material, a calcium-series top slag modifier is added after tapping is finished, and then a small platform is adopted for entering a station to feed an aluminum-magnesium wire for final deoxidation; the invention discloses a smelting method of steel for an ultrahigh-strength precision welded pipe, which comprises the steps of (S1) carrying out alloying on molten steel obtained in the step (S2), (S3) carrying out an LF process on the molten steel obtained in the step (S3), (S5) carrying out an RH process on the molten steel obtained in the step (S4), and (S6) feeding a Ca-Al core-spun yarn after alloying in the RH process, carrying out soft argon blowing, and carrying out continuous casting after the steel leaves a station. The smelting method of the steel for the ultrahigh-strength precision welded pipe provided by the invention can effectively control inclusions of a finished product, and realizes smelting of high-quality and high-cleanliness steel types.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a method for smelting steel for ultra-high strength precision welded pipes. Background Art

[0002] With the improvement of relevant laws and regulations in my country and the improvement of people's safety and environmental awareness, the energy conservation, emission reduction and safety performance of automobiles are increasingly valued. Therefore, the development and application of high-strength steel and ultra-high-strength steel, improving automobile safety, reducing automobile weight, achieving automobile lightweighting and reducing fuel consumption are the development trends of modern automobiles. As an emerging technology to achieve automobile lightweighting, high-strength steel meets the market demand well with its characteristics of light weight, high strength, good forming performance and high dimensional accuracy. Ultra-high strength precision welded pipe steel usually uses low-alloy, boron-containing steel, such as 62MnB5, 34MnB5, etc. Its microstructure after hot forming is a complete martensitic structure, with a yield strength of ≥1000MPa, a tensile strength of ≥1500MPa, a total elongation of ≥5%, good strength and wear resistance, high dimensional accuracy, and can be used for complex parts processing.

[0003] Ultra-high strength welded pipe steel is mainly used for fatigue structural products such as stabilizer bars and half shafts. During the early research, preparation and use, this type of steel is very easy to crack in the subsequent processing due to inclusions. This is also a common problem in the production of this type of steel at home and abroad.

[0004] At present, this type of steel generally uses aluminum deoxidation to remove alumina inclusions. There are three main methods to remove alumina inclusions: one is to blow argon into the ladle to strengthen the stirring of the molten steel and promote the floating of inclusions, but this method is time-consuming and requires white slag operation. There is a risk of silicon return when producing low-silicon steel; the second is to feed calcium alloys into the molten steel to modify the alumina inclusions. However, due to the active nature of calcium, it is very easy to gasify at steelmaking temperature, resulting in a low calcium recovery rate during calcium treatment, only 10%~20%; at the same time, calcium treatment has high requirements for the sulfur content in the steel (≤0.008%, or even lower); secondly, the amount of calcium added is difficult to control, and excessive addition of calcium will cause the steel to be oxidized and the sulfur content will be increased. Too little can not play a good modification role, too much will not only react with the sulfur in the molten steel to form CaS inclusions to block the water inlet, but also react with the refractory material of the ladle wall to produce new inclusions, which will greatly increase the cost of smelting and the modification effect is not ideal; the third is to remove inclusions through vacuum circulation, which is the same as the first method, both of which are physical modes to remove inclusions, but the inclusion removal efficiency is higher than the first method, and the effective removal rate is about 40%, which can meet the needs of general high-level steel grades. However, in the actual production process of this steel grade, using such conventional process conditions, the inclusions still cannot fully meet the requirements (rating higher than 1.5), and there is still a high proportion of cracking.

[0005] Therefore, in order to effectively remove inclusions from steel for ultra-high strength precision welded pipes, the applicant believes that the overall technical ideas are as follows: (1) reduce the deoxidation product Al2O3; (2) change the size of the deoxidation product to generate small particles and more diffusely distributed inclusions that are different from the conventional aluminum deoxidation clusters and large particles; (3) perform inclusion modification treatment after the refining treatment; however, how to effectively implement it still needs further exploration. Summary of the invention

[0006] The technical problem solved by the present invention is to provide a smelting method for steel for ultra-high strength precision welded pipes. The smelting method of the present application can effectively control inclusions and make the inclusions finer.

[0007] In view of this, the present application provides a method for smelting steel for ultra-high strength precision welded pipes, comprising the following steps:

[0008] S1) pre-treating molten iron to obtain semi-steel; wherein Cu≤0.10wt%, Mo≤0.05wt%, Ni≤0.10wt%, Sn≤0.03wt% in the molten iron;

[0009] S2) performing preliminary smelting of the semi-steel in a converter to obtain molten steel, wherein S of the semi-steel is ≤ 0.002wt%, C of the molten steel is 0.05-0.08wt%, and P is ≤ 0.006wt%;

[0010] S3) blowing argon into the molten steel during the whole process of tapping, adding lime to the mixture after 2 / 3 of the steel is tapped, and alloying is performed, adding a calcium-based top slag modifier after the steel is tapped, and then using a small platform to enter the station to feed the aluminum-magnesium line for final deoxidation;

[0011] S4) subjecting the molten steel obtained in step S3) to a LF process, wherein the target chemical composition is: C 0.30-0.40wt%, Si 0.15-0.35wt%, Mn 1.20-1.50wt%, P≤0.008wt%, S≤0.003wt%, Als 0.035-0.045wt%, Cr 0.010-0.020wt%, and the balance is Fe;

[0012] S5) subjecting the molten steel obtained in step S4) to a RH process, wherein the target chemical composition is: C 0.30-0.40wt%, Si 0.15-0.35wt%, Mn 1.20-1.50wt%, P≤0.008wt%, S≤0.003wt%, Als 0.02-0.06wt%, Cr 0.010-0.020wt%, Ti 0.020-0.040wt%, N≤0.0040wt%, B 0.0015-0.0035wt%, and the balance is Fe;

[0013] S6) After alloying in the RH process, the Ca-Al cored wire is fed, and then soft-blown with argon gas before exiting the station for continuous casting.

[0014] Preferably, in step S3), the amount of lime added is 5-7 kg / ton of steel; the alloying adopts low-nitrogen carbonaceous material for carbon alloying, with a target of 0.30wt%-0.32wt%, high-carbon ferromanganese with manganese, with a target of 1.15-1.25wt%, and high-carbon ferrochrome with chromium, with a target of 0.010-0.015wt%.

[0015] Preferably, the calcium-based top slag modifier includes: CaC2 30wt%~50wt%, Al2O3 10wt%~30wt%, CaO 20wt%~40wt%, CaF2 8wt%~15wt%, S≤0.2wt%, P≤0.1wt%.

[0016] Preferably, in step S3), the content of magnesium in the aluminum-magnesium wire is 5-15wt%, the content of aluminum is 85-95wt%, soft argon is blown throughout the process of feeding the aluminum-magnesium wire, the speed of feeding the aluminum-magnesium wire is 3-5m / s, and the feeding of the aluminum-magnesium wire is stopped when Als in the molten steel reaches 0.050wt%±0.010wt%, and the aluminum-magnesium wire is fed and soft argon is blown for ≥5min before leaving the station.

[0017] Preferably, in step S4), the molten steel in the LF process is soft-blown with argon for 6 to 8 minutes before leaving the station.

[0018] Preferably, in step S5), in the RH process, RH≤3mbar is circulated for 15-20min.

[0019] Preferably, in step S6), the Ca-Al cored wire contains 55-60wt% Ca and 40-45wt% Al, the specific gravity ratio of the Ca-Al cored wire to the iron sheet is ≥1 / 3, the feed amount is 0.3-0.6kg / t molten steel, and the wire feeding speed is 3-5m / s.

[0020] Preferably, in step S6), the soft blowing of argon gas is carried out after 10 to 12 minutes.

[0021] Preferably, the superheat degree of the molten steel in the continuous casting is 20-30° C., the continuous casting adopts medium-carbon low-alloy steel protection and a small chamfered crystallizer, and the reduction amount is 3-5 mm.

[0022] Preferably, the continuous casting speed is 1.0-1.5 m / min.

[0023] The present application provides a smelting method for steel for ultra-high strength precision welded pipes, which comprises the following steps: firstly, pre-treating molten iron to obtain semi-steel, and then performing primary smelting of the semi-steel in a converter to obtain molten steel, and then blowing argon through the molten steel to produce steel, and then sequentially performing LF process, RH process and continuous casting to obtain steel for ultra-high strength precision welded pipes; in the above process, the present application adopts full-process argon blowing to produce steel, so as to achieve the effect of suppressing nitrogen absorption during the steel-producing process, and at the same time, a small platform adopts a magnesium-aluminum alloy wire for final deoxidation, and while the magnesium-aluminum wire reduces the oxygen in the liquid steel, the deoxidation product generated by the magnesium-aluminum wire is finer than the single aluminum deoxidation product, and the inclusion control of the final product is more powerful, so that the inclusions are finer and more dispersed, and more suitable for the smelting of high-quality and high-cleanliness steel grades. DETAILED DESCRIPTION

[0024] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0025] In view of the problem that the inclusions in the ultra-high strength precision welded pipe steel in the prior art cannot meet the requirements, the present application provides a smelting method for ultra-high strength precision welded pipe steel, which achieves effective control of inclusions in the finished product through the whole process of argon blowing and final deoxidation of small platform magnesium-aluminum alloy wire, and obtains the smelting of high-quality and high-cleanliness steel. Specifically, the embodiment of the present invention discloses a smelting method for ultra-high strength precision welded pipe steel, comprising the following steps:

[0026] S1) pre-treating molten iron to obtain semi-steel; wherein Cu≤0.10wt%, Mo≤0.05wt%, Ni≤0.10wt%, Sn≤0.03wt% in the molten iron;

[0027] S2) performing preliminary smelting of the semi-steel in a converter to obtain molten steel, wherein S of the semi-steel is ≤ 0.002wt%, C of the molten steel is 0.05-0.08wt%, and P is ≤ 0.006wt%;

[0028] S3) blowing argon into the molten steel during the whole process of tapping, adding lime to the mixture after 2 / 3 of the steel is tapped, and alloying is performed, adding a calcium-based top slag modifier after the steel is tapped, and then using a small platform to enter the station to feed the aluminum-magnesium line for final deoxidation;

[0029] S4) subjecting the molten steel obtained in step S3) to a LF process, wherein the target chemical composition is: C 0.30-0.40wt%, Si 0.15-0.35wt%, Mn 1.20-1.50wt%, P≤0.008wt%, S≤0.003wt%, Als 0.035-0.045wt%, Cr 0.010-0.020wt%, and the balance is Fe;

[0030] S5) subjecting the molten steel obtained in step S4) to a RH process, wherein the target chemical composition is: C 0.30-0.40wt%, Si 0.15-0.35wt%, Mn 1.20-1.50wt%, P≤0.008wt%, S≤0.003wt%, Als 0.02-0.06wt%, Cr 0.010-0.020wt%, Ti 0.020-0.040wt%, N≤0.0040wt%, B 0.0015-0.0035wt%, and the balance is Fe;

[0031] S6) After alloying in the RH process, the Ca-Al cored wire is fed, and then soft-blown with argon gas before exiting the station for continuous casting.

[0032] The smelting method of the ultra-high strength precision welded pipe steel provided in this application is applicable to 34MnB5, and its composition requirements are shown in Table 1;

[0033] Table 1 Composition data of 34MnB5

[0034]

[0035] Molten iron was first prepared according to the composition of 34MnB5, with the following requirements: Cu≤0.10wt%, Mo≤0.05wt%, Ni≤0.10wt%, Sn≤0.03wt%; more specifically, Cu≤0.065wt%, Mo≤0.030wt%, Ni≤0.042wt%, Sn≤0.026wt%.

[0036] The present application performs vanadium extraction and desulfurization pretreatment on the molten iron to obtain semi-steel.

[0037] According to the present invention, the semi-steel is then initially smelted in a converter to obtain molten steel. The semi-steel is preferably initially smelted in a top and bottom double-blown converter, and the semi-steel is initially smelted into molten steel by utilizing the decarburization function of the top and bottom double-blown converter. In the present application, the S of the semi-steel entering the converter is ≤0.002wt%, the C at the converter end is 0.05~0.08wt%, and the end point P is ≤0.006wt%. Specifically, the S of the semi-steel is ≤0.001wt%, the C at the converter end is 0.051~0.075wt%, and the end point P is ≤0.0052wt%.

[0038] In the present application, argon is blown into the molten steel during the whole process to produce steel, and active lime is added after 2 / 3 of the steel is produced. The amount of active lime added is 5-7 kg / ton of steel. Specifically, the amount of active lime added is 5 kg / ton of steel, 6 kg / ton of steel or 7 kg / ton of steel. The steel is not deoxidized and alloyed. Specifically, low-nitrogen carbonaceous materials ([N]≤0.2%) are used for carbon alloying, with a target of 0.30-0.32% (combined with high carbon ferromanganese and manganese for carbon increase), and the carbon yield is considered to be 85%-87%; high carbon ferromanganese is used with manganese, with a target of 1.15%-1.25%, and a reference yield of 95%; high carbon ferrochrome is used with chromium, with a target of 0.010%-0.015%, and a reference yield of 95%.

[0039] After the steel is tapped, a calcium-based top slag modifier is added to the slag surface; the calcium-based top slag modifier includes: CaC2 30wt%~50wt%, Al2O3 10wt%~30wt%, CaO 20wt%~40wt%, CaF2 8wt%~15wt%, S≤0.2wt%, P≤0.1wt%; specifically, the calcium-based top slag modifier includes: CaC2 33wt%~48wt%, Al2O3 13wt%~27wt%, CaO2 4wt%~38wt%, CaF2 10wt%~13wt%, S≤0.2wt%, P≤0.1wt%; more specifically, the calcium-based top slag modifier includes: CaC2 37wt%~43wt%, Al2O3 15wt%~21wt%, CaO 27wt%~32wt%, CaF2 11wt%~12wt%, S≤0.2wt%, P≤0.1wt%. After that, a small platform is used to enter the station to feed the aluminum-magnesium wire for final deoxidation; in this process, the magnesium content in the aluminum-magnesium wire is 5-15wt%, and the aluminum content is 85-95wt%. Specifically, the magnesium content is 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, and the aluminum content is 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt%, 93wt%, 94wt%; during the feeding of the aluminum-magnesium wire, soft argon is blown throughout the process, and the speed of feeding the aluminum-magnesium wire is 3-5m / s. When Als in the molten steel reaches 0.050wt%±0.010wt%, the aluminum-magnesium wire is stopped from being fed, and the aluminum-magnesium wire is softly blown for ≥5min before exiting the station; specifically, the speed of feeding the aluminum-magnesium wire is 3m / s, 4m / s or 5m / s. During the wire feeding process, the ladle is softly blown with argon throughout the process, and the slag surface fluctuates, but the molten steel does not expose the slag surface. After final deoxidation, the Als content in the molten steel is 0.050±0.010%.

[0040] The present application then subjects the molten steel obtained above to a LF process for desulfurization, initial alloying adjustment and temperature compensation. The LF process is a process well known to those skilled in the art, and the present application does not impose any particular limitation on its specific implementation means. The target chemical composition after the LF process is: C 0.30~0.40wt%, Si 0.15~0.35wt%, Mn 1.20~1.50wt%, P≤0.008wt%, S≤0.003wt%, Als 0.035~0.045wt%, Cr 0.010~0.020wt%, and the balance is Fe; specifically, the target chemical composition is: C 0.31~0.37wt%, Si 0.18~0.32wt%, Mn 1.29~1.45wt%, P≤0.008wt%, S≤0.003wt%, Als 0.038~0.042wt%, Cr 0.013~0.018wt%, and the balance is Fe; more specifically, the target chemical composition is: C 0.32~0.35wt%, Si 0.19~0.25wt%, Mn 1.32~1.42wt%, P≤0.008wt%, S≤0.003wt%, Als0.039~0.041wt%, Cr 0.014~0.016wt%, and the balance is Fe.

[0041] According to the present invention, before the molten steel in the LF process leaves the station, it is soft-blown with a small argon flow rate for 6 to 8 minutes, and the argon flow rate is based on the molten steel being turned over without being exposed.

[0042] The present application then performs a RH process, wherein the RH≤3mbar is cycled for 15-20min, more specifically, the cycle is for 16-18min. The target chemical composition of the RH process is: C 0.30~0.40wt%, Si 0.15~0.35wt%, Mn 1.20~1.50wt%, P≤0.008wt%, S≤0.003wt%, Als 0.02~0.06wt%, Cr 0.010~0.020wt%, Ti0.020~0.040wt%, N≤0.0040wt%, B 0.0015~0.0035wt%, and the balance is Fe; specifically, the target chemical composition is: C 0.32~0.37wt%, Si 0.18~0.30wt%, Mn 1.22~1.46wt%, P≤0.008wt%, S≤0.003wt%, Als 0.033~0.050wt%, Cr 0.013~0.018wt%, Ti 0.025~0.038wt%, N≤0.0040wt%, B 0.0018~0.0033wt%, and the balance is Fe; more specifically, C 0.33~0.35wt%, Si 0.20~0.26wt%, Mn 1.31~1.42wt%, P≤0.008%, S≤0.003wt%, Als 0.038~0.045wt%, Cr 0.014~0.016wt%, Ti 0.028~0.035wt%, N≤0.0040wt%, B 0.0020~0.0030wt%, and the balance is Fe.

[0043] After the alloying in the RH process is completed, the Ca-Al cored wire is fed, and then soft-blown with argon for 10-12 minutes before leaving the station. The argon flow rate is based on the molten steel being turned over and not exposed. The Ca-Al cored wire contains 55-60wt% Ca and 40-45wt% Al, and the specific gravity ratio of the Ca-Al cored wire to the iron sheet is ≥1 / 3. The feeding amount is 0.3-0.6kg / t molten steel, and the wire feeding speed is 3-5m / s. Specifically, the Ca content in the Ca-Al cored wire is 56%, 57%, 58%, 59%, and the Al content is 41%, 42%, 43%, 44%, the feeding amount of the Ca-Al cored wire is 0.4kg / t molten steel, 0.5kg / t molten steel, and the wire feeding speed is 3m / s, 4m / s or 5m / s.

[0044] The present application finally carries out continuous casting, and the superheat of the molten steel during continuous casting is 20-30°C, and the continuous casting adopts medium-carbon low-alloy steel protection and a small chamfered crystallizer, the reduction is 3-5mm, and the pulling speed is 1.0-1.5m / min; specifically, the superheat is 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, and 29°C, the reduction is 3mm, 4mm, or 5mm, and the pulling speed is 1.1m / min, 1.2m / min, 1.3m / min, and 1.4m / min.

[0045] In order to further understand the present invention, the smelting method of steel for ultra-high strength precision welded pipe provided by the present invention is described in detail below in combination with embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0046] Example 1

[0047] (1) The vanadium-containing molten iron is obtained by smelting vanadium-titanium magnetite in a blast furnace. The residual elements of the molten iron entering the steel plant are Cu: 0.051wt%, Mo: 0.024wt%, Ni: 0.041wt%, and Sn: 0.025wt%;

[0048] (2) subjecting the above molten iron to vanadium extraction and desulfurization pretreatment to obtain semi-steel, which contains, by weight percentage, 3.56% C, 0.041% Mn, 0.064% P, 0.001% S, 0.03% V and trace amounts of Cr, Si and Ti, and residual elements Cu: 0.061%, Mo: 0.025%, Ni: 0.041%, Sn: 0.024%; the balance is iron and unavoidable impurities;

[0049] (3) adding 233.5 tons of the semi-steel into a 220-ton (nominal capacity) top-bottom combined blowing converter, and using the oxygen blowing and decarburization function of the top-bottom combined blowing converter to initially refine the semi-steel into molten steel. When the molten steel is initially refined to a C content of 0.051wt%, a Mn content of 0.033wt%, a P content of 0.0059wt%, a S content of 0.0025wt%, and a temperature of 1659° C., tapping of the thick slag into the ladle begins;

[0050] (4) Argon is blown throughout the steel tapping process, and 5 kg / t of active lime is added to the ladle after 2 / 3 of the steel is tapped;

[0051] (5) Steel is not deoxidized, and low-nitrogen carbonaceous materials ([N]: 0.18%) are used for carbon alloying, with a target of 0.30wt%; high-carbon ferromanganese with manganese, with a target of 1.15wt%; high-carbon ferrochromium with chromium, with a target of 0.010wt%;

[0052] (6) After steel tapping, add 3kg / t of calcium-based top slag modifier (CaC2 30%, Al2O3 30%, CaO 24%, CaF2 15%, S ≤ 0.2%, P ≤ 0.1%, and the rest are unavoidable impurities); the small platform enters the station to feed the aluminum-magnesium wire (Mg 5%, Al 95%) for final deoxidation, Als in the steel: 0.045%, soft blowing for 6 minutes before leaving the station;

[0053] (7) After that, it enters the LF process for desulfurization and alloying. Its chemical composition is shown in Table 2. Before the LF molten steel leaves the station, it is soft-blown with a small argon flow rate for 6 minutes. During the soft-blowing process, the molten steel is turned over and not exposed.

[0054] Table 2 LF alloy composition data after fine-tuning / wt%

[0055]

[0056] (8) Then enter the RH process, RH≤3mbar, cycle treatment time 15min; the chemical composition of the RH process is shown in Table 3;

[0057] Table 3 Chemical composition data of RH process treatment / wt%

[0058]

[0059] (9) After the alloying in the RH process, 0.6 kg / t of molten steel of Ca-Al cored wire (Ca 55%, Al 45%) was fed. Before the molten steel left the station, it was soft-blown with a small argon flow rate for 10 minutes. During the soft-blowing process, the molten steel was turned over and not exposed.

[0060] (10) Continuous casting is carried out after the RH process. The superheat of the molten steel in the continuous casting is 21°C. Medium carbon low alloy steel protective slag, small chamfered crystallizer, light pressure reduction (pressure reduction of 5mm) and casting speed of 1.2m / min are used for continuous casting. The inspection of the finished product samples obtained by continuous casting is shown in Table 4;

[0061] Table 4 Finished product composition data table / wt%

[0062]

[0063] The results of the rolled material inclusion detection are shown in Table 5;

[0064] Table 5 Rolled product inclusion rating data table

[0065]

[0066] Example 2

[0067] (1) The vanadium-containing molten iron is obtained by smelting vanadium-titanium magnetite in a blast furnace. The residual elements of the molten iron entering the steel plant are Cu: 0.062%, Mo: 0.021%, Ni: 0.034%, and Sn: 0.020%;

[0068] (2) subjecting the above molten iron to vanadium extraction and desulfurization pretreatment to obtain semi-steel, which contains, by weight percentage, 3.48% C, 0.032% Mn, 0.063% P, 0.002% S, 0.026% V, and trace amounts of Cr, Si and Ti, and residual elements Cu: 0.051%, Mo: 0.023%, Ni: 0.031%, Sn: 0.018%; the balance is iron and unavoidable impurities;

[0069] (3) adding 228.5 tons of the semi-steel into a 220-ton (nominal capacity) top-bottom combined blowing converter, and smelting the semi-steel into molten steel by using the oxygen blowing and decarburization function of the top-bottom combined blowing converter. When the molten steel is initially smelted to a C content of 0.071wt%, a Mn content of 0.036wt%, a P content of 0.0060wt%, a S content of 0.0028wt% and a temperature of 1665°C, tapping of the thick slag into the ladle begins;

[0070] (4) Argon is blown throughout the steel tapping process, and 6 kg / t of active lime is added to the ladle after 2 / 3 of the steel is tapped;

[0071] (5) Steel is not deoxidized, and low nitrogen carbonaceous materials ([N]: 0.18%) are used for carbon alloying, with a target of 0.30%; high carbon ferromanganese with manganese, target: 1.20%, high carbon ferrochrome with chromium, target: 0.012%;

[0072] (6) After steel tapping, add 4kg / t of calcium-based top slag modifier (CaC2 50%, Al2O3 21%, CaO 20%, CaF2 8%, S ≤ 0.2%, P ≤ 0.1%, and the rest are unavoidable impurities); the small platform enters the station to feed the aluminum-magnesium wire (Mg 15%, Al 85%) for final deoxidation, Als in the steel: 0.040%, soft blowing for 7 minutes before exiting the station;

[0073] (7) After that, it enters the LF process for desulfurization and alloying. Its chemical composition is shown in Table 6. Before the LF molten steel leaves the station, it is soft-blown with a small argon flow rate for 6 minutes. During the soft-blowing process, the molten steel is turned over and not exposed.

[0074] Table 6 LF alloy composition data after fine-tuning / wt%

[0075]

[0076] (8) Then enter the RH process, RH≤3mbar, cycle treatment time 18min; the chemical composition of the RH process is shown in Table 7;

[0077] Table 7 Chemical composition data of RH process treatment / wt%

[0078]

[0079] (9) After the alloying in the RH process is completed, 0.45 kg / t of Ca-Al cored wire (Ca 60%, Al 40%) is fed into the molten steel; before the molten steel leaves the station, it is soft-blown with a small argon flow rate for 11 minutes, and the molten steel is turned over during the soft-blowing process without being exposed;

[0080] (10) Continuous casting was carried out after the RH process. The superheat of the molten steel in the continuous casting was 22°C. Medium carbon low alloy steel protective slag, small chamfered crystallizer, light pressure reduction (pressure reduction of 5 mm), and casting speed of 1.1 m / min were used for continuous casting. The inspection of the finished product samples obtained by continuous casting is shown in Table 8.

[0081] Table 8 Finished product composition data table / wt%

[0082]

[0083] The results of the rolled material inclusion detection are shown in Table 9;

[0084] Table 9 Rolled product inclusion rating data table

[0085]

[0086] Example 3

[0087] (1) The vanadium-containing molten iron is obtained by smelting vanadium-titanium magnetite in a blast furnace. The residual elements of the molten iron entering the steel plant are Cu: 0.055%, Mo: 0.026%, Ni: 0.041%, and Sn: 0.026%;

[0088] (2) subjecting the above molten iron to vanadium extraction and desulfurization pretreatment to obtain semi-steel, which contains, by weight percentage, 3.56% C, 0.041% Mn, 0.052% P, 0.002% S, 0.03% V, and trace amounts of Cr, Si and Ti, and residual elements Cu: 0.053%, Mo: 0.024%, Ni: 0.039%, Sn: 0.024%; the remainder is iron and unavoidable impurities;

[0089] (3) adding 230.7 tons of the semi-steel into a 220-ton (nominal capacity) top-bottom combined blowing converter, and using the oxygen blowing and decarburization function of the top-bottom combined blowing converter to initially refine the semi-steel into molten steel. When the molten steel is initially refined to a C content of 0.075wt%, a Mn content of 0.031wt%, a P content of 0.0052wt%, a S content of 0.0020wt%, and a temperature of 1668°C, tapping of the thick slag into the ladle begins;

[0090] (4) Argon is blown throughout the steel tapping process, and 7kg / t of active lime is added to the ladle after 2 / 3 of the steel is tapped;

[0091] (5) Steel is not deoxidized, and low nitrogen carbonaceous materials ([N]: 0.18%) are used for carbon alloying, with a target of 0.30%; high carbon ferromanganese with manganese, target: 1.25%, high carbon ferrochrome with chromium, target: 0.015%;

[0092] (6) After steel tapping, add 5kg / t of calcium-based top slag modifier (CaC2 30%, Al2O3 13%, CaO 40%, CaF2 15%, S ≤ 0.2%, P ≤ 0.1%, and the rest are unavoidable impurities); the small platform enters the station to feed the aluminum-magnesium wire (Mg 5%, Al 95%), Als in the steel: 0.050%, soft blowing for 5 minutes before exiting the station;

[0093] (7) After that, it enters the LF process for desulfurization and alloying. Its chemical composition is shown in Table 10. Before the LF molten steel leaves the station, it is soft-blown with a small argon flow rate for 6 minutes. During the soft-blowing process, the molten steel is turned over and not exposed.

[0094] Table 10 LF alloy composition data after fine-tuning / wt%

[0095]

[0096] (8) Then enter the RH process, RH≤3mbar, cycle treatment time 20min; the chemical composition of the RH process is shown in Table 11;

[0097] Table 11 Chemical composition data of RH process treatment / wt%

[0098]

[0099] (9) After the alloying in the RH process, 0.45 kg / t of molten steel of Ca-Al cored wire (Ca 55%, Al 45%) was fed. Before the molten steel left the station, it was soft-blown with a small argon flow rate for 11 minutes. During the soft-blowing process, the molten steel was turned over and not exposed.

[0100] (10) Continuous casting is carried out after the RH process. The superheat of the molten steel in the continuous casting is 27°C. Medium carbon low alloy steel protective slag, small chamfered crystallizer, light pressure reduction (pressure reduction of 5mm) and casting speed of 1.1m / min are used for continuous casting. The inspection of the finished product samples obtained by continuous casting is shown in Table 12;

[0101] Table 12 Finished product composition data table / wt%

[0102]

[0103] The results of the rolled material inclusion detection are shown in Table 13;

[0104] Table 13 Rolled product inclusion rating data table

[0105]

[0106] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0107] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A smelting method for ultra-high strength precision welded pipe steel, comprising the following steps: S1) pre-treating molten iron to obtain semi-steel; wherein Cu≤0.10wt%, Mo≤0.05wt%, Ni≤0.10wt%, Sn≤0.03wt% in the molten iron; S2) performing preliminary smelting of the semi-steel in a converter to obtain molten steel, wherein S of the semi-steel is ≤ 0.002wt%, C of the molten steel is 0.05-0.08wt%, and P is ≤ 0.006wt%; S3) blowing argon into the molten steel during the whole process of tapping, adding lime to the mixture after 2 / 3 of the steel is tapped, and alloying is performed, adding a calcium-based top slag modifier after the steel is tapped, and then using a small platform to enter the station to feed the aluminum-magnesium line for final deoxidation; S4) subjecting the molten steel obtained in step S3) to a LF process, wherein the target chemical composition is: C 0.30-0.40wt%, Si 0.15-0.35wt%, Mn 1.20-1.50wt%, P≤0.008wt%, S≤0.003wt%, Als 0.035-0.045wt%, Cr 0.010-0.020wt%, and the balance is Fe; S5) subjecting the molten steel obtained in step S4) to a RH process, wherein the target chemical composition is: C 0.30-0.40wt%, Si 0.15-0.35wt%, Mn 1.20-1.50wt%, P≤0.008wt%, S≤0.003wt%, Als 0.02-0.06wt%, Cr 0.010-0.020wt%, Ti 0.020-0.040wt%, N≤0.0040wt%, B 0.0015-0.0035wt%, and the balance is Fe; S6) After alloying in the RH process, the Ca-Al cored wire is fed, and then soft-blown with argon gas before exiting the station for continuous casting.

2. The smelting method according to claim 1, characterized in that: In step S3), the amount of lime added is 5-7 kg / ton of steel; the alloying adopts low-nitrogen carbonaceous materials for carbon alloying, with a target of 0.30wt%-0.32wt%, high-carbon ferromanganese with manganese, with a target of 1.15-1.25wt%, and high-carbon ferrochrome with chromium, with a target of 0.010-0.015wt%.

3. The smelting method according to claim 1, characterized in that: The calcium-based top slag modifier includes: CaC2 30wt%~50wt%, Al2O3 10wt%~30wt%, CaO 20wt%~40wt%, CaF2 8wt%~15wt%, S≤0.2wt%, P≤0.1wt%.

4. The smelting method according to claim 1, characterized in that: In step S3), the content of magnesium in the aluminum-magnesium wire is 5-15wt%, the content of aluminum is 85-95wt%, soft argon is blown throughout the process of feeding the aluminum-magnesium wire, the speed of feeding the aluminum-magnesium wire is 3-5m / s, and the feeding of the aluminum-magnesium wire is stopped when Als in the molten steel reaches 0.050wt%±0.010wt%, and the aluminum-magnesium wire is fed and soft argon is blown for ≥5min before leaving the station.

5. The smelting method according to claim 1, characterized in that: In step S4), the molten steel in the LF process is soft-blown with argon for 6 to 8 minutes before leaving the station.

6. The smelting method according to claim 1, characterized in that: In step S5), in the RH process, RH≤3mbar is circulated for 15-20min.

7. The smelting method according to claim 1, characterized in that: In step S6), the Ca-Al cored wire contains 55-60wt% Ca and 40-45wt% Al, the specific gravity ratio of the Ca-Al cored wire to the iron sheet is ≥1 / 3, the feeding amount is 0.3-0.6kg / t molten steel, and the wire feeding speed is 3-5m / s.

8. The smelting method according to claim 1, characterized in that: In step S6), the soft blowing of argon gas is completed after 10-12 minutes.

9. The smelting method according to claim 1, characterized in that: The superheat degree of the molten steel in the continuous casting is 20-30° C. The continuous casting adopts medium-carbon low-alloy steel protection and a small chamfered crystallizer, and the reduction amount is 3-5 mm.

10. The smelting method according to claim 1, characterized in that: The continuous casting speed is 1.0-1.5 m / min.