Power angle steel for low-alloy high-strength high-toughness Q460C iron tower and preparation method of power angle steel

By using the preparation method of low alloy high strength and high toughness Q460C tower electric angle steel in the steel for power transmission tower, the problems of insufficient steel strength and high production cost in the existing technology are solved, and high yield strength, tensile strength and impact toughness are achieved. , and reduce production costs and meet the load-bearing capacity requirements of high load and high altitude towers.

CN119040761AActive Publication Date: 2024-11-29SHANDONG SHIHENG SPECIAL STEEL GROUP

Patent Information

Application Number
CN202411160190.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The strength value of existing steel for power transmission towers is relatively low, resulting in large steel consumption and high production costs, low-temperature impact toughness cannot be stable and qualified, making it difficult to meet the load-bearing capacity requirements of high-load and high-altitude towers.

Method used

The grain size and structure of the steel billet are controlled by using low alloy high strength and high toughness Q460C towers and their preparation methods. Structure, reduce the addition of alloy elements and improve the purity and strength of steel.

Benefits of technology

The high yield strength, tensile strength and impact toughness of the angle steel used in Q460C towers has been achieved, which reduces production costs, improves the economic and social benefits of steel, and meets the load-bearing capacity requirements of high load and high-altitude towers.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of steel for power transmission towers, in particular to low-alloy high-strength high-toughness electric angle steel for a Q460C iron tower and a preparation method of the electric angle steel. The preparation method at least comprises the steps of billet heating, rolling forming and cooling. In the steel billet heating step, the temperature of a first heating section is controlled to be 900-1030 DEG C, the temperature of a second heating section is controlled to be 1150-1250 DEG C, the temperature of a soaking section is controlled to be 1140-1240 DEG C, and the tapping temperature of a steel billet is controlled to be 1050-1160 DEG C; in the rolling forming step, double-BD rolling and finish rolling four-continuous rolling are adopted, the steel waiting temperature is controlled before finish rolling, and the initial rolling temperature of finish rolling is 800-900 DEG C; and an ultrafast cooling device is adopted in the cooling step. According to the angle steel for the Q460C iron tower, a microalloying component system is adopted, and a specific controlled rolling and controlled cooling process is matched, so that the strength and impact toughness of the finally obtained angle steel for the Q460C iron tower can exceed the standard requirements, the angle steel has large surplus, and the production cost is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel for power transmission towers, and in particular to a low-alloy high-strength and high-toughness Q460C power angle steel for power transmission towers and a preparation method thereof. Background Art

[0002] At present, the main materials of steel used for power transmission towers in my country are generally Q355 and Q420, and the diagonal materials are mainly Q235 and Q355. The strength values ​​of these steels used for power transmission towers are relatively low, so the steel consumption of power transmission line towers is relatively large. There are more and more double-circuit towers, multi-circuit towers, and spanning towers. The height of the towers is increasing, and the load of the towers is increasing; the application of multiple split conductors has greatly increased the load of the towers. This development trend puts higher requirements on the carrying capacity of power transmission towers. At the same time, it also requires that the tower weight and corridor area of ​​the power transmission towers be reduced and minimized as much as possible.

[0003] Improving the mechanical properties of steel used for transmission towers is an effective means to improve the bearing capacity of transmission towers and reduce the weight of towers. The production of angle steels at home and abroad adopts conventional rolling process, without controlled rolling and controlled cooling process, and the structure is generally ferrite + pearlite. It is basically ensured by adding microalloys such as Nb, V, Ti, etc. to ensure strength and toughness. The production cost is high, and the low-temperature impact toughness cannot be stably qualified. The smelting and rolling production efficiency is extremely low, and the smelting cost remains high. Prior art CN 109127724 A provides a production process method for high-toughness angle steel, which performs air-drying treatment on the steel plate after rough and medium rolling to reduce the temperature of the steel plate when entering the finishing mill, so that the medium and large-sized angle steels above ∠10 produce deformation-induced ferrite precipitation during finishing rolling, which promotes grain refinement. This prior art can improve the impact toughness of medium and large-sized angle steels, but does not have the effect of improving the yield strength and tensile strength of the angle steels. Summary of the invention

[0004] Aiming at the problem that the current power angle steels of transmission towers are mostly of QA235, Q355 and Q420 models and their mechanical properties need to be improved, the present invention provides a low-alloy high-strength and high-toughness Q460C power angle steel for towers and a preparation method thereof.

[0005] In a first aspect, the present invention provides a method for preparing low-alloy high-strength and high-toughness Q460C power angle steel for iron towers, which comprises at least the steps of heating the steel billet, rolling forming and cooling; The chemical composition of the steel billet is calculated by weight percentage, including C 0.14%~0.18%, Si 0.25%~0.40%, Mn 1.35%~1.50%, V 0.04%~0.08%, P≤0.025%, S≤0.02%, Als 0.015%~0.03%, N≤0.015%, and the balance is Fe and unavoidable impurities; In the billet heating step, the temperature of the first heating stage is controlled to be 900-1030°C, the furnace pressure of the first heating stage is 20±10Pa, the temperature of the second heating stage is 1150-1250°C, the furnace pressure of the second heating stage is 25±10Pa, the temperature of the soaking stage is 1140-1240°C, the furnace pressure of the soaking stage is 30±10Pa, and the billet out-of-furnace temperature is 1050-1160°C; The rolling forming step adopts double BD rolling + four-pass finishing rolling, the BD1 starting rolling temperature is 1050~1150℃, rolling 5 times, BD2 rolling 3 times, BD2 final rolling temperature is 1000~1100℃, the steel temperature is controlled before finishing rolling, the finishing rolling starting rolling temperature is 800~900℃, rolling 4 times, and the finishing rolling final rolling temperature is 780~850℃; The cooling step uses an ultra-fast cooling device, and the temperature of the angle steel after cooling is 640~685℃.

[0006] Furthermore, the steel billet is selected from a square cross-section steel billet or a rectangular cross-section steel billet, for example, a square steel billet with a size of 165mm×165mm, a rectangular steel billet with a cross-section size of 180mm×220mm, or a rectangular steel billet with a cross-section size of 220mm×290mm is obtained by continuous casting.

[0007] Furthermore, the billet heating time is 50 to 60 minutes.

[0008] Furthermore, the temperature control time of the steel before finish rolling is 50~90s, and the temperature is reduced by 150~250℃.

[0009] Furthermore, the finishing rolling speed is 1-1.5 m / s.

[0010] Furthermore, the main pipe pressure of the ultra-fast cooling device is 9~11bar, and the flow rate is 800~900m 3 / h, the frequency is 40~50Hz, and the ultra-fast cold roller speed is 1~1.5m / s.

[0011] Furthermore, it also includes converter smelting and continuous casting steps. The converter smelting adopts efficient dephosphorization technology, improves the early oxidizability of the converter, adopts slag retention operation to quickly form early slag process technology, adopts high-drawing and blowing process to improve the converter dephosphorization rate, the molten steel is refined in LF furnace, silicon carbide and ferrosilicon powder are used for diffusion deoxidation, and aluminum addition operation is performed after the free oxygen content in the molten steel is lower than 5ppm. The Als content of the molten steel is controlled at 0.015%~0.030%, and a high-basicity ternary slag system is produced to absorb calcium aluminate inclusions generated after adding aluminum, which can not only ensure the recovery rate of aluminum elements, but also reduce Al 2 O 3 The formation of inclusions is conducive to smooth pouring of continuous casting; The continuous casting adopts protective pouring, compound flow control + stopper rod automatic control, electromagnetic stirring, and ultra-weak cooling system during the pouring process; Through the above-mentioned converter smelting and continuous casting steps, the obtained steel billet has high steel purity, few defects, and has the characteristics of low production cost, high safety and strong practicality.

[0012] In a second aspect, the present invention provides a low-alloy, high-strength and high-toughness Q460C electric angle steel for iron towers produced by the above-mentioned preparation method.

[0013] Furthermore, the grain size grade of the low-alloy high-strength and high-toughness Q460C power angle steel for iron towers reaches above grade 8.5, the yield strength is between 490~545MPa, the tensile strength is between 600~655MPa, the longitudinal impact toughness at 0℃ is 80~120J, and the elongation after fracture is >22%.

[0014] The beneficial effects of the present invention are: The present invention adopts a micro-alloying component system and cooperates with a specific controlled rolling and controlled cooling process to achieve reduced addition of alloy elements such as Mn and V, save expensive alloys, and reduce the requirements for steel purity (mainly inclusions in the components). The strength and impact toughness of the Q460C angle steel for iron towers finally obtained can exceed the standard requirements with a large margin, and the production cost is greatly reduced.

[0015] The Q460C angle steel for iron tower of the present invention has reasonable composition and process design, loose production control and process system, and can be stably produced on the profile line. Based on the production of 2,000 tons of Q460C power angle steel for iron tower in one year, the profit per ton of steel is more than 600 yuan, and the annual profit can reach more than 1.2 million yuan, which has high economic benefits. At the same time, the production process is simple, the energy consumption is low, and it is green and low-carbon, which has positive social benefits.

[0016] The steel billet heating step of the present invention adopts micro-positive pressure control, adopts a shorter heating time and a lower rolling start temperature, and can effectively control the original austenite grain size of the steel billet; the double BD rolling is both rolled in the austenite recrystallization zone, and the austenite grains as fine as possible are obtained through repeated deformation-recrystallization; the finishing rolling process promotes the precipitation of VN at the austenite grain boundary and in the crystal by controlling the temperature of the steel; in the ultra-fast cooling process, a large amount of ferrite can be generated at the austenite grain boundary and in the crystal with VN particles as the core, thereby increasing the nucleation driving force of ferrite during phase transformation, refining the final organization, and thus improving the strength and toughness of the steel. DETAILED DESCRIPTION

[0017] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0018] Example 1 A low-alloy high-strength and high-toughness Q460C power angle steel for iron tower is produced according to the following preparation method: (1) Converter smelting Adopt high-efficiency dephosphorization technology, improve the early oxidation of converter, adopt slag retention operation to quickly form early slag process technology, adopt high-drawing supplementary blowing process to improve converter dephosphorization rate, molten steel is refined by LF furnace, silicon carbide and ferrosilicon powder are used for diffusion deoxidation, and aluminum addition operation is carried out after the free oxygen content in molten steel is lower than 5ppm to make high-basicity ternary slag system, absorb calcium aluminate inclusions generated after aluminum addition, which can not only ensure the recovery rate of aluminum element, but also reduce Al 2 O 3 The formation of inclusions is conducive to smooth pouring of continuous casting.

[0019] (2) Continuous casting By adopting protective pouring, compound flow control + stopper rod automatic control, electromagnetic stirring and ultra-weak cooling system in the pouring process, high-purity Q460C qualified 220mm×290mm rectangular billet is obtained, with chemical composition of C 0.15%, Si 0.33%, Mn1.35%, V 0.054%, P 0.018%, S 0.008%, Als 0.03%, N 0.011%, and the balance is Fe and unavoidable impurities.

[0020] (3) Billet heating The temperature of the first heating stage is controlled to be 1010℃, the furnace pressure of the first heating stage is 18Pa, the temperature of the second heating stage is 1205℃, the furnace pressure of the second heating stage is 21Pa, the temperature of the soaking section is 1150℃, the furnace pressure of the soaking section is 22Pa, the billet is heated for 58min, and the billet out of the furnace temperature is 1100℃.

[0021] (4) Rolling forming Rolling of ∠200×20 equal-leg angle steel adopts double BD rolling + four-continuous finishing rolling. The starting rolling temperature of BD1 is 1100℃, and it is rolled for 5 passes. After two 90° steel turnings, BD2 is rolled for 3 passes, and the final rolling temperature of BD2 is 1000℃. The BD2 extension roller controls the temperature of the steel for 55s. The finishing rolling entrance temperature is 900℃, and it is rolled for 4 passes. The final rolling temperature of finishing rolling is 850℃. The rolling speed is controlled to be 1m / s during the finishing rolling process.

[0022] (5) Cooling The ultra-fast cooling device (SH00-00-00) is used to control the main pipe pressure to 10.2 bar and the flow rate to 850m 3 / h, 2 pumps are turned on, the frequency is 43Hz, the ultra-fast cold roller speed is 1.1m / s, and the temperature of the angle steel after cooling is 645℃.

[0023] The grain size and mechanical properties of the Q460C power angle steel for iron tower obtained in Example 1 were tested. The grain size grade of the angle steel was 9.0, the yield strength was 545 MPa, the tensile strength was 655 MPa, the longitudinal impact toughness at 0°C was 144 J, and the elongation after fracture was 25%.

[0024] The Q460C electric angle steel for iron tower obtained in Example 1 is observed. After the controlled cooling step, the surface of the electric angle steel forms a metallographic structure mainly composed of pearlite + ferrite + bainite, and the metallographic structure of the core of the electric angle steel is mainly pearlite + ferrite.

[0025] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not perform controlled cooling, and naturally cools after rolling.

[0026] The angle steel obtained in Example 1 was tested for grain size and mechanical properties. The grain size grade of the angle steel was 7.5, the yield strength was 470 MPa, the tensile strength was 585 MPa, the longitudinal impact toughness at 0°C was 85 J, and the elongation after fracture was 26%.

[0027] The grain size of Comparative Example 1 is coarser than that of Example 1, which is the main reason for the low impact toughness. The low performance is mainly due to the lack of controlled cooling process, the absence of bainite structure in the organization, and only pearlite and ferrite. Under the same composition conditions, the performance is 75MPa lower in yield strength and 70MPa lower in tensile strength than that of the embodiment of the present invention.

[0028] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the converter smelting step in Comparative Example 2 does not perform aluminum addition operation, and the chemical composition of the steel billet is C 0.15%, Si 0.33%, Mn 1.35%, V 0.054%, P 0.018%, S 0.008%, N 0.011%, and the balance is Fe and unavoidable impurities.

[0029] The angle steel obtained in Comparative Example 2 was tested for grain size and mechanical properties. The angle steel had a grain size of 8.0, a yield strength of 530 MPa, a tensile strength of 645 MPa, a longitudinal impact toughness of 52 J at 0°C, and an elongation of 24%.

[0030] Since no Al element is added to the composition of Comparative Example 2, the grain size is coarse, which is the main reason for the low impact toughness. Due to the controlled cooling process, the performance is basically consistent with the embodiment of the present invention.

[0031] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the finishing rolling temperature of Comparative Example 3 is 920°C, and the temperature of the angle steel after cooling is 500°C.

[0032] The angle steel obtained in comparative example 3 was tested for grain size and mechanical properties. The angle steel had a grain size of 9.5, a yield strength of 580 MPa, a tensile strength of 705 MPa, a longitudinal impact toughness of 135 J at 0°C, and an elongation of 17%.

[0033] In Comparative Example 3, the final rolling temperature is relatively high, the temperature after controlled cooling is relatively low, and the cooling intensity increases, which increases the bainite content in the structure of the angle steel, increases the depth of the hardened layer, and tempered martensite and tempered troostite appear in some positions, resulting in increased yield strength and tensile strength, and a sharp decrease in elongation after fracture, which is not conducive to the application of power angle steel in iron towers.

[0034] Example 2 A low-alloy high-strength and high-toughness Q460C power angle steel for iron tower is produced according to the following preparation method: (1) Converter smelting Adopt high-efficiency dephosphorization technology, improve the early oxidation of converter, adopt slag retention operation to quickly form early slag process technology, adopt high-drawing supplementary blowing process to improve converter dephosphorization rate, molten steel is refined by LF furnace, silicon carbide and ferrosilicon powder are used for diffusion deoxidation, and aluminum addition operation is carried out after the free oxygen content in molten steel is lower than 5ppm to make high-basicity ternary slag system, absorb calcium aluminate inclusions generated after aluminum addition, which can not only ensure the recovery rate of aluminum element, but also reduce Al 2 O 3 The formation of inclusions is conducive to smooth pouring of continuous casting.

[0035] (2) Continuous casting By adopting protective pouring, compound flow control + stopper rod automatic control, electromagnetic stirring and ultra-weak cooling system in the pouring process, high-purity Q460C qualified 220mm×290mm rectangular billet is obtained. The chemical composition is C 0.16%, Si 0.36%, Mn1.36%, V 0.050%, P 0.024%, S 0.014%, Als 0.026%, N 0.012%, and the balance is Fe and unavoidable impurities.

[0036] (3) Billet heating The temperature of the first heating stage is controlled to be 980℃, the furnace pressure of the first heating stage is 16Pa, the temperature of the second heating stage is 1180℃, the furnace pressure of the second heating stage is 18Pa, the temperature of the soaking section is 1150℃, the furnace pressure of the soaking section is 20Pa, the billet is heated for 60min, and the billet out of the furnace temperature is 1050℃.

[0037] (4) Rolling forming Rolling of ∠180×16 equilateral angle steel adopts double BD rolling + four-continuous finishing rolling. The starting rolling temperature of BD1 is 1050℃, and it is rolled for 5 passes. After two 90° steel turnings, BD2 is rolled for 3 passes, and the final rolling temperature of BD2 is 980℃. The BD2 extension roller controls the temperature of the steel for 65s. The finishing rolling entrance temperature is 890℃, and it is rolled for 4 passes. The final rolling temperature of finishing rolling is 850℃. The rolling speed is controlled at 1.3m / s during the finishing rolling process.

[0038] (5) Cooling The ultra-fast cooling device (SH00-00-00) is used to control the main pipe pressure to 9.5 bar and the flow rate to 800m 3 / h, 2 pumps are turned on, the frequency is 41Hz, the ultra-fast cold roller speed is 1.5m / s, and the temperature of the angle steel after cooling is 650℃.

[0039] The grain size and mechanical properties of the Q460C electric angle steel for iron tower obtained in Example 2 were tested. The grain size grade of the angle steel was 9.0, the yield strength was between 530 MPa, the tensile strength was between 650 MPa, the longitudinal impact toughness at 0°C was 96 J, and the elongation after fracture was 24%.

[0040] Observe the Q460C electric angle steel for iron tower obtained in Example 2. After the controlled cooling step, the surface of the electric angle steel forms a metallographic structure mainly composed of pearlite + ferrite + bainite, and the metallographic structure of the core of the electric angle steel is mainly pearlite + ferrite.

[0041] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.

Claims

1. A method for preparing low-alloy high-strength and high-toughness Q460C power angle steel for iron tower, characterized in that: At least including the steps of billet heating, rolling forming and cooling; The chemical composition of the steel billet is calculated by weight percentage, including C 0.14%~0.18%, Si 0.25%~0.40%, Mn 1.35%~1.50%, V 0.04%~0.08%, P≤0.025%, S≤0.02%, Als 0.015%~0.03%, N≤0.015%, and the balance is Fe and unavoidable impurities; In the billet heating step, the temperature of the first heating stage is controlled to be 900-1030°C, the furnace pressure of the first heating stage is 20±10Pa, the temperature of the second heating stage is 1150-1250°C, the furnace pressure of the second heating stage is 25±10Pa, the temperature of the soaking stage is 1140-1240°C, the furnace pressure of the soaking stage is 30±10Pa, and the billet out-of-furnace temperature is 1050-1160°C; The rolling forming step adopts double BD rolling + four-pass finishing rolling, the BD1 starting rolling temperature is 1050~1150℃, rolling 5 times, BD2 rolling 3 times, BD2 final rolling temperature is 1000~1100℃, the steel temperature is controlled before finishing rolling, the finishing rolling starting rolling temperature is 800~900℃, rolling 4 times, and the finishing rolling final rolling temperature is 780~850℃; The cooling step uses an ultra-fast cooling device, and the temperature of the angle steel after cooling is 640~685℃.

2. The preparation method according to claim 1, characterized in that The steel billet is selected from a square cross-section steel billet or a rectangular cross-section steel billet.

3. The preparation method according to claim 1, characterized in that: The billet heating time is 50~60min.

4. The preparation method according to claim 1, characterized in that: The steel temperature control time before finishing rolling is 50~90s.

5. The preparation method according to claim 1, characterized in that: The finishing rolling speed is 1~1.5m / s.

6. The preparation method according to claim 1, characterized in that: The main pipe pressure of the ultra-fast cooling device is 9~11bar, and the flow rate is 800~900m 3 / h, the frequency is 40~50Hz, and the ultra-fast cold roller speed is 1~1.5m / s.

7. The preparation method according to claim 1, characterized in that: It also includes converter smelting and continuous casting steps. The molten steel is refined in an LF furnace, and diffusion deoxidation is carried out using silicon carbide and ferrosilicon powder. After the free oxygen content in the molten steel is lower than 5ppm, aluminum addition operation is carried out, and the Als content of the molten steel is controlled at 0.015%~0.030%.

8. A low alloy high strength and high toughness Q460C power angle steel for iron tower produced by the preparation method as claimed in claim 1.

9. The low alloy high strength and high toughness Q460C power angle steel for iron tower as claimed in claim 8, characterized in that: The grain size grade reaches above 8.5, the yield strength is between 490~545MPa, the tensile strength is between 600~655MPa, the longitudinal impact toughness at 0℃ is 80~120J, and the elongation after fracture is >22%.

Citation Information

Patent Citations

  • Rolling method of high-toughness low-alloy high-strength steel

    CN113215492A

Cited By

  • Power angle steel for high-precision iron tower and production method of power angle steel

    CN120174256A