Biphase compound coating and preparation method thereof

The preparation of the biphasic compound CoxCrFezNb0.3NiSiYmC0.5 coating through high-energy ball milling and plasma cladding processes has solved the problem of insufficient hardness and wear resistance in the prior art, and achieved the coordinated strengthening effect of high hardness and wear resistance, and expanded the The application range of coatings.

CN119040876AInactive Publication Date: 2024-11-29HENAN POLYTECHNIC INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411162758.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing coating technology has shortcomings in improving workpiece hardness and wear resistance, especially in complex working conditions, it is difficult to meet the performance requirements of multi-compound coatings.

Method used

The two-phase compound CoxCrFezNb0.3NiSiYmC0.5 coating was prepared by a combination of high-energy ball milling and plasma cladding. The wear resistance of the coating was improved by forming the two-phase structure of FCC1 and FCC2 and the coordinated strengthening of diamond particles.

Benefits of technology

It significantly improves the hardness and wear resistance of the workpiece, forms a unique crystal structure, expands the application range of compound coatings, and is highly productive and easy to produce in industrial use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040876A_ABST
    Figure CN119040876A_ABST
Patent Text Reader

Abstract

The invention discloses a dual-phase compound coating and a preparation method thereof, and belongs to the field of compound preparation. According to the method, the CoxCrFezNb0. 3NiSiYmC0.5 (x is more than or equal to 0.1 and less than or equal to 1.1) with a two-phase structure of FCC1 and FCC2 is prepared by adopting a process of combining high-energy ball milling and plasma cladding; 0.1 < = z < = 1; 0.1 < = m < = 0.5; 0.01 lt; 0.01 lt; x / (x + z + m + 3.8) lt; 0.23, 0.23; 0.01 lt; 0.01 lt; z / (x + z + m + 3.8) lt; 0.20, 0.20; 0.01 lt; 0.01 lt; m / (x + z + m + 3.8) lt; and 0.10) a compound coating. According to the CoxCrFezNb0. 3NiSiYmC0. 5 compound coating prepared through the method, metallurgical bonding can be formed between the coating and a base body, a synergistic strengthening effect can be formed between the coating and diamond particles, and the wear resistance of the coating is further improved; the hardness of the prepared coating can reach up to 3200Hv, and the coating is good in wear resistance, high in production efficiency and easy for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of compound preparation, and in particular relates to a dual-phase compound coating and a preparation method thereof. Background Art

[0002] As a common surface treatment method, coating technology can significantly improve the specific performance of the substrate surface under certain working conditions, thereby achieving the purpose of extending the service life of the workpiece, enhancing the performance, and improving the efficiency of use. There are many types of coating preparation methods, and the common methods are: chemical vapor deposition (CVD), physical vapor deposition (PVD), cladding method, etc. Chemical vapor deposition is to place the workpiece to be processed into a deposition chamber filled with reactive gas, and then decompose it at high temperature to form the required target coating on the surface of the workpiece. Common CVD coatings include: titanium nitride, titanium carbonitride, aluminum oxide, etc. Physical vapor deposition can evaporate or sputter the target material into a gas state at a lower temperature, and then deposit a coating of the target component on the surface of the workpiece. Common PVD coatings include: diamond-like coating, titanium aluminum nitride coating, nano multilayer structure coating, etc. Common cladding methods for preparing coatings mainly include laser cladding and plasma cladding. Ceramic particles or other carbide particles can be embedded in the metal matrix to form a composite coating, which can significantly improve the wear resistance and corrosion resistance of the workpiece surface. As a new type of coating, multi-component compound coating can not only form a new crystal structure different from the constituent elements of the compound due to its large variety of elements, but also can generate gradient functional coatings in situ during the solidification process, and often exhibits good physical and chemical properties. In addition, a reinforcing phase with a certain specific function can be added during the preparation of the multi-component coating by the cladding method. While forming a metallurgical bond between the surface of the workpiece substrate and the coating, a composite coating containing a specific reinforcing phase evenly distributed in the coating can be formed. The preparation of a compound with a completely new crystal structure for the coating can not only enrich the theory of compound component design and preparation, but also expand the application range of the compound coating, which has important theoretical significance and use value. Therefore, the design and preparation of a two-phase compound coating has broad market prospects. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a dual-phase compound Co x CrFe z Nb 0.3 NeA m C 0.5 Coating and method for preparing the same.

[0004] The dual-phase compound Co proposed in the present invention x CrFe z Nb 0.3 NeA m C0.5 Coating and its preparation method, a duplex compound is prepared by a process combining high-energy ball milling and plasma cladding, and the chemical formula of the compound is Co x CrFe z Nb 0.3 NiSiY m C 0.5 , and the compound is a two-phase structure composed of FCC1 (face-centered cubic structure, space group Fd-3m(227), lattice constant 1.083021 nm) and FCC2 (face-centered cubic structure, space group Fd-3m(227), lattice constant 1.075854 nm); the prepared Co x CrFe z Nb 0.3 NiSiY m C 0.5 coating is uniform and can greatly improve the hardness and wear resistance of the workpiece.

[0005] The technical solution of the present invention is realized as follows: a preparation method of a duplex compound coating, which is characterized by the following steps:

[0006] (1) According to the chemical formula of the compound coating Co x CrFe z Nb 0.3 NiSiY m C 0.5 , where 0.1 ≤ x ≤ 1.1; 0.1 ≤ z ≤ 1; 0.1 ≤ m ≤ 0.5; 0.01 < x / (x + z + m + 3.8) < 0.23; 0.01 < z / (x + z + m + 3.8) < 0.20; 0.01 < m / (x + z + m + 3.8) < 0.10; respectively weigh the required metal powder, silicon powder and diamond powder, and place the above raw material powders in a vacuum ball milling tank for high-energy ball milling;

[0007] (2) Take out the powder after high-energy ball milling in a protective gas environment, and modulate it with 97 wt% turpentine alcohol and 3 wt% ethyl cellulose into a paste-like precursor, prefabricate the precursor on the substrate and dry it;

[0008] (3) Perform plasma cladding on the substrate prefabricated with the precursor in step (2), and the duplex Co x CrFe z Nb 0.3 NiSiY m C 0.5 compound coating is obtained after the cladding is completed.

[0009] In the step (1), the purities of the metal powder, silicon powder and diamond powder are all higher than 99.5%.

[0010] The high-energy ball milling process in step (1) is as follows: the time is 0.5h to 2h, and the rotation speed is 150rpm to 200rpm.

[0011] In the step (2), the protective gas is argon or nitrogen.

[0012] In the step (2), the substrate material is 45 steel or Q235 steel.

[0013] The drying process in step (2) is as follows: the temperature is 80° C. to 120° C., and the insulation time is 1 h to 6 h.

[0014] The plasma cladding process in step (3) is as follows: current 120-140A, cladding voltage 34V, plasma arc moving speed 120-180mm / min.

[0015] The beneficial effects of the present invention are as follows: (1) the present invention adopts a plasma cladding process to add diamond reinforcement phase particles to the coating, and the prepared coating can not only form a gradient functional coating with metallurgical bonding with the substrate, but also form a synergistic strengthening effect with the diamond particles, thereby further improving the wear resistance of the coating; (2) the Co prepared by the present invention has a two-phase structure consisting of FCC1 (face-centered cubic structure, space group is Fd-3m (227), lattice constant is 1.083021nm) and FCC2 (face-centered cubic structure, space group is Fd-3m (227), lattice constant is 1.075854nm) x CrFe z Nb 0.3 NeA m C 0.5 The crystal structure formed by the compound used in the prepared coating is different from that of each constituent element, which not only enriches the design theory of new compound components, but also expands the application scope of the compound coating; (3) The coating prepared by the present invention has a hardness of up to 3200Hv, good wear resistance, high production efficiency, and is easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the X-ray diffraction pattern of the dual-phase compound coating prepared in Example 1.

[0017] Figure 2 This is a photo of the dual-phase compound coating prepared in Example 1. DETAILED DESCRIPTION

[0018] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0019] Example 1

[0020] According to the compound coating chemical formula CoCrFeNb0.3 NeA 0.1 C 0.5 0.40 mol of cobalt powder, chromium powder, iron powder, nickel powder, silicon powder, 0.12 mol of niobium powder, 0.04 mol of yttrium powder and 0.20 mol of diamond powder were weighed respectively, and the purity of the above powders was higher than 99.5%; and the above raw material powders were placed in a vacuum ball mill for high-energy ball milling, the ball milling time was 0.5 h, and the rotation speed was 200 rpm; the powder after high-energy ball milling was taken out under an argon environment, and mixed with 97 wt% of turpentine alcohol and 3 wt% of ethyl cellulose to form a paste precursor, and the precursor was prefabricated on a 45 steel substrate and dried at a drying temperature of 80° C. and a heat preservation time of 6 h; the substrate of the prefabricated precursor was plasma clad, the cladding current was 140 A, the cladding voltage was 34 V, and the plasma arc moving speed was 180 mm / min; after the cladding was completed, a dual-phase CoCrFeNb 0.3 NeA 0.1 C 0.5 Compound coating.

[0021] Example 2

[0022] According to the compound coating chemical formula Co 1.1 CrFe 0.5 Nb 0.3 NeA 0.1 C 0.5 0.44 mol of cobalt powder, 0.40 mol of chromium powder, nickel powder, silicon powder, 0.20 mol of iron powder, diamond powder, 0.12 mol of niobium powder and 0.04 mol of yttrium powder were weighed respectively, and the purity of the above powders was higher than 99.5%; and the above raw material powders were placed in a vacuum ball mill for high-energy ball milling, the ball milling time was 1.5 hours, and the rotation speed was 170 rpm; the powder after high-energy ball milling was taken out under a nitrogen environment, and mixed with 97 wt% of turpentine and 3 wt% of ethyl cellulose to form a paste precursor, and the precursor was prefabricated on a Q235 steel substrate and dried at a drying temperature of 100 ° C and a heat preservation time of 4 hours; the substrate of the prefabricated precursor was plasma clad, the cladding current was 130A, the cladding voltage was 34V, and the plasma arc moving speed was 150mm / min; after the cladding was completed, a dual-phase Co 1.1 CrFe 0.5 Nb 0.3 NeA 0.1 C 0.5 Compound coating.

[0023] Example 3

[0024] According to the compound coating chemical formula Co 0.3 CrFe 0.1 Nb 0.3 NeA0.2 C 0.5 0.12mol of cobalt powder, niobium powder, 0.40mol of chromium powder, nickel powder, silicon powder, 0.04mol of iron powder, 0.08mol of yttrium powder and 0.20mol of diamond powder were weighed respectively, and the purity of the above powders was higher than 99.5%; and the above raw material powders were placed in a vacuum ball mill for high-energy ball milling, the ball milling time was 2h, and the rotation speed was 150rpm; the powder after high-energy ball milling was taken out under an argon environment, and was modulated into a paste precursor with 97wt% of turpentine alcohol and 3wt% of ethyl cellulose, and the precursor was prefabricated on a 45 steel substrate and dried at a drying temperature of 120°C and a holding time of 1h; the substrate of the prefabricated precursor was plasma clad, the cladding current was 120A, the cladding voltage was 34V, and the plasma arc moving speed was 120mm / min; after the cladding was completed, a dual-phase Co 0.3 CrFe 0.1 Nb 0.3 NeA 0.2 C 0.5 Compound coating.

[0025] Example 4

[0026] According to the compound coating chemical formula Co 0.1 CrFeNb 0.3 NeA 0.3 C 0.5 0.04 mol of cobalt powder, 0.40 mol of chromium powder, iron powder, nickel powder, silicon powder, 0.12 mol of niobium powder, yttrium powder and 0.20 mol of diamond powder were weighed respectively, and the purity of the above powders was higher than 99.5%; and the above raw material powders were placed in a vacuum ball mill for high-energy ball milling, the ball milling time was 0.5 h, and the rotation speed was 200 rpm; the powder after high-energy ball milling was taken out under an argon environment, and mixed with 97 wt% of turpentine alcohol and 3 wt% of ethyl cellulose to form a paste precursor, and the precursor was prefabricated on a 45 steel substrate and dried at a drying temperature of 80° C. and a heat preservation time of 6 h; the substrate of the prefabricated precursor was plasma clad, the cladding current was 140 A, the cladding voltage was 34 V, and the plasma arc moving speed was 180 mm / min; after the cladding was completed, a dual-phase Co 0.1 CrFeNb 0.3 NeA 0.3 C 0.5 Compound coating.

[0027] Example 5

[0028] According to the compound coating chemical formula Co 0.5 CrFe 0.3 Nb 0.3 NeA 0.3 C 0.50.20 mol of cobalt powder, diamond powder, 0.40 mol of chromium powder, nickel powder, silicon powder and 0.12 mol of iron powder, niobium powder and yttrium powder were weighed respectively, and the purity of the above powders was higher than 99.5%; and the above raw material powders were placed in a vacuum ball mill for high-energy ball milling, the ball milling time was 1.5 hours, and the rotation speed was 170 rpm; the powder after high-energy ball milling was taken out under a nitrogen environment, and mixed with 97 wt% of turpentine and 3 wt% of ethyl cellulose to form a paste precursor, and the precursor was prefabricated on a Q235 steel substrate and dried at a drying temperature of 100 ° C and a heat preservation time of 4 hours; the substrate of the prefabricated precursor was plasma clad, the cladding current was 130A, the cladding voltage was 34V, and the plasma arc moving speed was 150mm / min; after the cladding was completed, a dual-phase Co 0.5 CrFe 0.3 Nb 0.3 NeA 0.3 C 0.5 Compound coating.

[0029] Example 6

[0030] According to the compound coating chemical formula Co 1.1 CrFeNb 0.3 NeA 0.5 C 0.5 0.44 mol of cobalt powder, 0.40 mol of chromium powder, iron powder, nickel powder, silicon powder, 0.12 mol of niobium powder and 0.20 mol of yttrium powder and diamond powder were weighed respectively, and the purity of the above powders was higher than 99.5%; and the above raw material powders were placed in a vacuum ball mill for high-energy ball milling, the ball milling time was 2 hours, and the rotation speed was 150 rpm; the powder after high-energy ball milling was taken out under an argon environment, and mixed with 97 wt% of turpentine alcohol and 3 wt% of ethyl cellulose to form a paste precursor, and the precursor was prefabricated on a 45 steel substrate and dried at a drying temperature of 120° C. and a heat preservation time of 1 hour; the substrate of the prefabricated precursor was plasma clad, the cladding current was 120A, the cladding voltage was 34V, and the plasma arc moving speed was 120 mm / min; after the cladding was completed, a dual-phase Co 1.1 CrFeNb 0.3 NeA 0.5 C 0.5 Compound coating.

Claims

1. A method for preparing a dual-phase compound coating, characterized in that The compound coating is Co x CrFe z Nb 0.3 NiSiY m C 0.5 , where 0.1 ≤ x ≤ 1.1; 0.1 ≤ z ≤ 1; 0.1 ≤ m ≤ 0.5; 0.01 < x / (x + z + m + 3.8) < 0.23; 0.01 < z / (x + z + m + 3.8) < 0.20; 0.01 < m / (x + z + m + 3.8) < 0.10; and the compound of the coating is a two-phase structure composed of FCC1 (face-centered cubic structure, space group Fd-3m(227), lattice constant 1.083021 nm) and FCC2 (face-centered cubic structure, space group Fd-3m(227), lattice constant 1.075854 nm) Co x CrFe z Nb 0.3 NiSiY m C 0.5 compound, and the preparation method of the compound coating comprises the following steps: (1) According to the chemical formula of the compound coating Co x CrFe z Nb 0.3 NiSiY m C 0.5 , where 0.1 ≤ x ≤ 1.1; 0.1 ≤ z ≤ 1; 0.1 ≤ m ≤ 0.5; 0.01 < x / (x + z + m + 3.8) < 0.23; 0.01 < z / (x + z + m + 3.8) < 0.20; 0.01 < m / (x + z + m + 3.8) < 0.10; Weigh the required metal powder, silicon powder and diamond powder respectively, and place the above raw material powders in a vacuum ball milling tank for high-energy ball milling; (2) taking out the powder after high-energy ball milling under a protective gas environment, and mixing it with 97 wt % of turpentine alcohol and 3 wt % of ethyl cellulose to form a paste precursor, prefabricating the precursor on a substrate and drying it; (3) Plasma cladding is performed on the substrate of the precursor prepared in step (2), and a dual-phase Co x CrFe z Nb 0.3 NeA m C 0.5 Compound coating.

2. The method for preparing a dual-phase compound coating according to claim 1, characterized in that: In the step (1), the purity of the metal powder, silicon powder and diamond powder is higher than 99.5%.

3. The method for preparing a dual-phase compound coating according to claim 1, characterized in that: The high-energy ball milling process in step (1) is as follows: the time is 0.5h to 2h, and the rotation speed is 150rpm to 200rpm.

4. The method for preparing a dual-phase compound coating according to claim 1, characterized in that: In the step (2), the protective gas is argon or nitrogen.

5. The method for preparing a dual-phase compound coating according to claim 1, characterized in that: In the step (2), the substrate material is 45 steel or Q235 steel.

6. The method for preparing a dual-phase compound coating according to claim 1, characterized in that: The drying process in step (2) is as follows: the temperature is 80° C. to 120° C., and the insulation time is 1 h to 6 h.

7. The method for preparing a dual-phase compound coating according to claim 1, characterized in that: The plasma cladding process in step (3) is as follows: current 120-140A, cladding voltage 34V, plasma arc moving speed 120-180mm / min.