Laser-cladding high-hardness wear-resistant coating on surface of automobile brake disc and preparation method of laser-cladding high-hardness wear-resistant coating

By using laser cladding technology to form a high hard wear-resistant coating of NiCr-Cr3C2 composite powder and AlN powder on the surface of the automobile brake disc, the problem of insufficient hardness and wear resistance of the brake disc is solved, and the performance and use of the brake disc are significantly improved. Lifespan, while reducing environmental pollution.

CN119040883APending Publication Date: 2024-11-29SHANDONG JIANZHU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411283611.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The hardness of the car brake disc is low and the wear resistance is poor, resulting in a short service life and particle pollution during friction, affecting health and the environment.

Method used

Laser cladding technology is used to form a high hard wear-resistant coating of NiCr-Cr3C2 composite powder and AlN powder on the surface of the brake disc, and the hardness and wear resistance of the material are improved by metallurgical combination.

Benefits of technology

It significantly improves the hardness, wear resistance and oxidation resistance of the brake disc, extends the service life, and reduces processing costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040883A_ABST
    Figure CN119040883A_ABST
Patent Text Reader

Abstract

The invention relates to the field of metal surface modification, in particular to an automobile brake disc surface laser cladding high-hardness wear-resistant coating and a preparation method thereof, and solves the problems that an existing brake disc is low in hardness, poor in wear resistance, prone to plastic deformation and the like. Laser cladding powder is prepared, wherein the laser cladding powder comprises NiCr-Cr3C2 composite powder and AlN powder; the metal substrate is preheated, then laser cladding is carried out, and a high-hardness wear-resistant coating can be formed on the surface of the metal substrate. The process parameters are as follows: the laser power is 700-1000W, the powder feeding rate is 10-13g / min, the scanning speed is 5-10mm / s, the spot diameter is 2-4mm, the lap joint rate is 30-45%, argon with the purity of more than or equal to 99.9% is selected as laser cladding shielding gas, and the shielding gas flow is 10-15L / min. The coating obtained through the method has a compact tissue structure, the bonding strength with a matrix is high, and the surface is free of obvious defects such as air holes and cracks; the average hardness of the coating is not lower than 1000 HV, the wear rate is not higher than 4 * 10 <-6 > mm < 3 >, the compression ratio of a cladding sample is not higher than 42%, the bending strength is not lower than 1000 MPa, and the impact toughness is lower than 20 J. The grain boundary strength is improved, the coating density is high, and the coating has good hardness, abrasion resistance and deformation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material surface modification, and in particular to a laser-clad high-hardness and wear-resistant coating on the surface of an automobile brake disc and a preparation method thereof. Background Art

[0002] With the continuous development of the domestic automobile industry, brake discs have been widely used in automobile braking systems. Brake discs slow down or stop vehicles by friction with brake pads. The friction between brake discs and brake pads will not only cause wear of brake discs and reduce the service life of brake discs, but also cause fine particle pollution in urban areas, which seriously endangers health. As a key component of automobile braking system, the base material of automobile brake discs is mostly gray cast iron, while the base material of brake discs of high-end cars is more expensive, the manufacturing process is complex, and the production cost is high. In view of this, improving the performance of automobile brake discs through material surface modification technology is a very effective new way. In the field of material surface modification technology, the rapid development of laser cladding technology has opened up a new way to improve the performance of automobile parts. Laser cladding technology can be used to prepare a coating with dense structure, high surface quality and various excellent mechanical properties on the surface of cast iron. Compared with the base-layer combination prepared by traditional preparation process, the base and coating in laser cladding are metallurgical combination, and the prepared cladding layer has better overall performance.

[0003] It can be seen from this that improving the surface performance of the brake disc through laser cladding technology can not only improve the various properties of the brake disc such as wear resistance, increase the service life of the brake disc, and improve the cost performance, but the cladding process can also be realized in a short time, greatly reducing the processing time. Summary of the invention

[0004] The main purpose of the present invention: According to the current development trend in the field of surface modification technology, the present invention provides a laser-clad high-hardness and wear-resistant coating on the surface of an automobile brake disc and a preparation method thereof. The present invention has a simple manufacturing process, and uses laser cladding technology to clad a layer of high-hardness and wear-resistant coating on the surface of the brake disc. The coating obtained by the technical solution of the present invention is relatively thick, has excellent mechanical properties such as high hardness and high wear resistance, has fewer defects such as cracks and pores on the coating surface, and has a simple processing process, low processing cost, and is easy to produce. It is suitable for the use of brake discs in automobile braking systems and can be widely used in the automotive industry.

[0005] In order to improve the current problems of low hardness and poor wear resistance of brake discs, easy plastic deformation, etc., the present invention discloses a laser cladding high-hardness and wear-resistant coating on the surface of automobile brake discs and a preparation method thereof. The components and the mass percentage of each component are: NiCr-Cr 3 C 2Composite powder, 15-25wt% AlN powder. In the above powder, NiCr-Cr 3 C 2 The powder is a commonly used alloy composite powder, which has both metal phase NiCr and ceramic phase Cr 3 C 2 The advantages of both, Cr 3 C 2 It is a hard phase with high strength and resistance to high temperature oxidation, wear and corrosion. NiCr is a bonding phase, providing toughness and low thermal stress. NiCr will wrap around Cr. 3 C 2 , so NiCr-Cr 3 C 2 It has excellent comprehensive properties such as wear resistance, corrosion resistance and oxidation resistance at high temperatures. 3 C 2 The coating contains Cr 3 C 2 and Cr 7 C 3 Hard phase, which can improve wear resistance. NiCr-Cr 3 C 2 Since the composite powder contains a large amount of Cr element, it has strong hardness, excellent self-melting, wettability and bonding performance. 3 C 2 In the air, it will be severely oxidized at 1100℃~1400℃, because dense Cr 2 O 3 Protective film, the oxide film can hinder further oxidation, so Cr 3 C 2 It has strong corrosion resistance and wear resistance. 3 C 2 AlN ceramic powder is added to the composite powder. AlN powder has excellent wear resistance, corrosion resistance, high temperature stability and other properties. AlN powder is mixed with metal powder and a composite coating is prepared by laser cladding and other processes, which can significantly improve the mechanical properties and wear resistance of the material, and significantly enhance the hardness, strength and wear resistance of the metal material. 3 C 2 The composite powder forms an Al-Cr melt with AlN powder at high temperature. The high melting point Cr 3 C 2 It gradually dissolves with AlN to form an Al-Cr-CN molten pool; the solid solubility of C and N in the melt reaches the limit, and the Al element in the surrounding melt diffuses into the solid solution, significantly improving the hardness and wear resistance of the coating.

[0006] The present invention discloses a high-hardness and wear-resistant coating on the surface of a vehicle brake disc by laser cladding and a preparation method thereof, which is prepared according to the following method:

[0007] Step 1: Clean and pretreat the surface of the metal substrate (brake disc);

[0008] Step 2: Prepare the powder required for coating according to mass percentage. The powder includes NiCr-Cr 3 C 2 Composite powder, 15-25wt% AlN powder, the powder is mixed evenly and then dried to obtain laser cladding powder;

[0009] Step 3: Preheat the surface of the metal substrate to 200°C, and then use laser cladding technology to clad the powder on the surface of the metal substrate to form a high-hardness and wear-resistant coating on the surface of the metal substrate.

[0010] Among them, the metal substrate is selected as gray cast iron suitable for automobile brake discs. The coating can be adapted to the performance requirements of different materials by changing the composition ratio, laser process parameters, etc.

[0011] Preferably, the cleaning pretreatment in step 1 is to grind the cladding surface of the metal substrate with a grinder to make it smooth, then grind it with 100#-600# sandpaper in sequence to remove the surface oxide layer, and clean the polished surface with acetone and alcohol solution in sequence and dry it. Anhydrous ethanol can achieve a good cleaning effect. The metal substrate can be polished and cleaned according to the specific conditions of the metal substrate to ensure that the coating has a high bonding strength with the metal substrate during subsequent laser cladding.

[0012] Preferably, in step 2, the powder required for the coating is prepared by first accurately weighing the weight of each element powder using an electronic balance with an accuracy of 0.001g, and the weighed powder is mixed using a Wzm-10L mixer, the mixer speed is 250rad / min, the mixing time is 3 hours, and the mixed powder is dried in a drying oven for 2 hours, so that the powders are mixed evenly and the powders are prevented from being oxidized.

[0013] Preferably, the laser cladding technology process parameters in step 3 are: laser power 700-1000W, powder feeding rate 10-13g / min, scanning speed 5-10mm / s, spot diameter 2-4mm, overlap rate 30-45%, laser cladding shielding gas uses argon with a purity of ≥99.9%, and shielding gas flow rate 10-15L / min. When performing laser cladding operation, one of the coaxial powder feeding method and the pre-set powder method can be selected.

[0014] The technical solution provided by the present invention has the following advantages:

[0015] 1. The present invention creatively performs laser cladding modification on the surface of gray cast iron to form a cladding layer on the surface of the brake disc. The cladding layer has a high density, and the hardness and wear resistance are improved. The wear resistance, corrosion resistance, heat resistance, oxidation resistance and deformation resistance of the brake disc can be improved. The alloy layers are metallurgically bonded, have good bonding properties, are not easy to fall off, have a long service life, and the laser cladding process does not cause environmental pollution.

[0016] 2. The present invention improves the traditional cast iron hot processing by an effective process method. By using laser cladding technology, during the laser processing on the gray cast iron surface, the laser beam has high energy density, fast processing speed, and local processing, with no or little effect on the non-laser irradiated parts. The heat-affected zone is small, the workpiece has small thermal deformation, and the subsequent processing volume is small.

[0017] 3. The high-hardness and wear-resistant coating prepared by the present invention has a dense structure and is well bonded to the substrate. The average hardness of the prepared coating is not less than 1000 HV, and the wear rate is not higher than 4×10 -6 mm 3 The compression rate is not higher than 42%, the bending strength is not less than 1000MPa, the impact toughness is less than 20J, and the overall coating strength has been significantly improved compared with the original brake disc performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a graph of the average hardness of Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7 and the comparative example samples.

[0019] Figure 2 It is a wear rate diagram of Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7 and the comparative example sample.

[0020] Figure 3 It is a compression rate graph of Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7 and the comparative example sample.

[0021] Figure 4 This is a graph of the maximum bending strength of the coating samples of Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7 and the comparative example.

[0022] Figure 5 It is a graph of impact toughness of Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7 and comparative example samples.

[0023] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work. DETAILED DESCRIPTION

[0025] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0026] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0027] The raw materials used in the embodiments of the present invention are as follows: the particle size of NiCr / Cr3C2 powder is 45-105 μm, w(Ni)=24.8%; w(C)=8.64%; w(Si)=0.37%; w(Fe)=0.80%; w(Cr)=65.39%.

[0028] The specific composition of gray cast iron HT250 is: w(C)=2.6%~3.8%; w(Si)=1.2%~3.0%; w(Mn)=0.4%~1.2%; w(P)≤0.4%; w(S)≤0.15%; w(Fe)=91.45%~95.8%.

[0029] The embodiment of the present invention discloses a high-hardness and wear-resistant coating on the surface of a vehicle brake disc by laser cladding and a preparation method thereof, the steps of which are as follows:

[0030] Step 1: Clean and pretreat the surface of the metal substrate; use a grinder to grind the cladding surface of the metal substrate to make it smooth, then use 100#-600# sandpaper to grind it until it is bright to remove the surface oxide layer, and use acetone and alcohol solution to clean the polished surface and dry it. Anhydrous ethanol can achieve a good cleaning effect. The metal substrate can be polished and cleaned according to the specific situation of the metal substrate to ensure that the coating has a high bonding strength with the metal substrate during subsequent laser cladding.

[0031] Step 2: Prepare the powder required for coating according to mass percentage. The powder includes NiCr-Cr 3 C 2Composite powder, particle size is 45-105μm; 15-25wt% AlN powder, particle size is 53-150μm, the powders are mixed evenly and then dried to obtain laser cladding powder; firstly, the weight of each element powder is accurately weighed with an electronic balance with an accuracy of 0.001g, and the weighed powder is mixed with a Wzm-10L mixer, the mixer speed is 250rad / min, the mixing time is 3 hours, and the mixed powder is dried in a drying oven for 2 hours, so that the powders are mixed evenly and prevented from being oxidized.

[0032] Step 3: Preheat the surface of the metal substrate to 200°C, use coaxial powder feeding method, and the laser cladding technology process parameters are: laser power 700-1000W, powder feeding rate 10-13g / min, scanning speed 5-10mm / s, spot diameter 2-4mm, overlap rate 30-45%, laser cladding shielding gas uses argon with a purity of ≥99.9%, and the shielding gas flow rate is 10-15L / min.

[0033] The embodiment of the present invention discloses a high-hardness and wear-resistant coating on the surface of an automobile brake disc by laser cladding and a preparation method thereof, and the test indicators are: hardness test, friction and wear test, and material strength test.

[0034] Hardness test: The HVS-1000A microhardness tester was used to test the hardness of the cladding layer. The hardness tester load was 5N, the holding time was 15s, the interval between every two adjacent test points was 50μm, and the average value was taken for analysis.

[0035] Friction and wear test: 40N down force, 100rad / min speed of the testing machine, 30min wear time, GCr15 as the grinding specimen, and an analytical balance (with an accuracy of 0.0001g) were used to measure the mass of the sample before and after to obtain the average wear rate.

[0036] Material strength test: CMT5504 electronic universal testing machine was used to carry out room temperature compression test and bending test of the material. The material compression test was carried out under the conditions of load of 100kN and speed of 0.02mm / min, and the material bending test was carried out at a loading speed of 2mm / min. The compression rate and maximum bending strength of the coating sample were obtained respectively.

[0037] Impact toughness test: The impact toughness test was conducted using a JBN-300C microcomputer-controlled pendulum impact tester at room temperature. There was a V-shaped notch in the middle of the sample length, with an angle of 45°, a notch depth of 2mm, and a root radius of 0.25mm.

[0038] The specific embodiments of the present invention are described in detail below.

[0039] Example 1 A laser cladding high-hardness and wear-resistant coating on the surface of an automobile brake disc and a preparation method thereof, the steps are:

[0040] Step 1: Use gray cast iron as the base material, and clean and pre-treat the surface of the steel plate; the cleaning pre-treatment is to grind the cladding surface of the metal substrate with a grinder to make it smooth, and then use 100#-600# sandpaper to grind it to a bright finish to remove surface burrs, rust and oxide layers, and use acetone and alcohol solution to clean the polished surface and dry it to remove oxides and impurities on the surface of the metal substrate, and then dry it.

[0041] Step 2: Prepare the powder required for coating according to the mass fraction percentage. The powder includes NiCr-Cr 3 C 2 Composite powder, particle size is 45-105μm; 15-25wt% AlN powder, particle size is 53-150μm, the powders are mixed evenly and then dried to obtain laser cladding powder; firstly, the weight of each element powder is accurately weighed with an electronic balance with an accuracy of 0.001g, and the weighed powder is mixed with a Wzm-10L mixer, the mixer speed is 250rad / min, the mixing time is 3 hours, and the mixed powder is dried in a drying oven for 2 hours, so that the powders are mixed evenly and prevented from being oxidized.

[0042] Step 3: Preheat the surface of the metal substrate to 200°C, use coaxial powder feeding method, and the laser cladding technology process parameters are: laser power 700-1000W, powder feeding rate 10-13g / min, scanning speed 5-10mm / s, spot diameter 2-4mm, overlap rate 30-45%, laser cladding shielding gas uses argon with a purity of ≥99.9%, and the shielding gas flow rate is 10-15L / min.

[0043] Based on Example 1, Examples 2 to 7 were obtained by laser cladding. The results of the average hardness, wear rate, compression rate, maximum bending strength and impact toughness of the coatings obtained by performing hardness tests, friction and wear tests, compressive strength, tensile strength and impact toughness tests on the above Examples 1 to 7 are shown in the following table.

[0044] Table 1 Average hardness, average wear rate of cladding layer, compression rate, maximum bending strength and impact toughness of cladding specimens sample <![CDATA[Average hardness (HV 0.5 )]]> <![CDATA[Wear rate (×10 -6 mm 3 )]]> Compression rate (%) Flexural strength(MPa) Impact toughness(J) Example 1 1101.5 2.76 34.99 1266.76 21.3 Example 2 1055.2 3.99 34.25 1184.99 31.0 Example 3 1087.3 3.38 33.62 1367.82 24.1 Example 4 1189.1 2.43 33.56 1378.57 24.3 Example 5 1073.1 3.74 34.71 1365.40 29.5 Example 6 1123.8 2.62 34.88 1023.96 21.1 Example 7 1079.0 3.69 35.80 1276.90 26.4 Comparative Example (substrate) 357.8 20.8 41.09 398.00 15.8

[0045] The present invention discloses a method for preparing a high-hardness and wear-resistant coating on the surface of an automobile brake disc by laser cladding. It can be seen from the examples that the coating prepared by the present invention has good density, good bonding strength between the coating and a substrate, and the prepared coating has high hardness, wear resistance, compression resistance, bending strength and impact toughness. Therefore, the brake disc obtained by laser cladding technology has good strength, wear resistance, deformation resistance and impact damage resistance.

[0046] According to the average hardness of the samples, the high-hardness and wear-resistant coating prepared by laser cladding has an average hardness of 3.02 times that of the substrate. Compared with the substrate brake disc material itself, the cladding layer exhibits higher hardness.

[0047] According to the wear rate of the sample, the high-hardness and wear-resistant coating prepared on the brake disc surface by laser cladding technology has significantly improved the wear resistance of the cladding layer. The wear rate of the cladding layer of Example 4 is the smallest, so the wear resistance is the best.

[0048] According to the compression rate of the samples, the compression rate of each embodiment is about 34%, and the compression rate of the substrate is relatively large, exceeding 40%. Compared with the substrate, the cladding layer has higher compressive strength, and the compression resistance of the cladding layer is maintained in a relatively stable range.

[0049] According to the bending strength of the samples, the bending strength of the material has been significantly improved. Examples 3 to 7 have greater bending strength. Compared with the brake disc itself, the maximum bending strength is increased by 71.13%.

[0050] According to the impact toughness of the sample, the higher the impact toughness of the material, the better the ability to resist impact damage. It can be seen that the impact toughness of the sample after cladding has been significantly improved, so the ability to resist impact damage is better than that of the substrate.

Claims

1. A laser cladding high-hardness and wear-resistant coating on the surface of an automobile brake disc and a preparation method thereof, characterized in that: The mass percentage of the powder required for the coating is: NiCr-Cr3C2 composite powder, 15-25wt% AlN powder.

2. A laser cladding high-hardness and wear-resistant coating on the surface of an automobile brake disc and a preparation method thereof, characterized in that: The steps are: Step 1: Clean and pretreat the surface of the metal substrate; Step 2: Prepare the powder required for coating according to the mass percentage, the powder includes: NiCr-Cr3C2 composite powder, 15-25wt% AlN powder. Mix the powder evenly and dry it to obtain laser cladding powder; Step 3: Preheat the surface of the metal substrate to 200°C, and then use laser cladding technology to melt the powder onto the surface of the metal substrate to form a high-hardness and wear-resistant coating on the surface of the metal substrate.

3. The laser cladding high-hardness and wear-resistant coating on the surface of an automobile brake disc and the preparation method thereof according to claim 2, characterized in that: The two powders required for laser cladding in step 2 are: NiCr-Cr3C2 composite powder with a particle size of 45-105 μm; 15-25wt% AlN powder with a particle size of 53-150 μm.

4. The laser cladding high-hardness and wear-resistant coating on the surface of an automobile brake disc and the preparation method thereof according to claim 2, characterized in that: The cleaning pretreatment in step 1 is to grind the cladding surface of the metal substrate smooth with a grinder, then grind it with 100#-600# sandpaper in sequence until it is bright to remove the surface oxide layer, and clean the polished surface with acetone and alcohol solution in sequence and dry it.

5. The laser cladding high-hardness and wear-resistant coating on the surface of an automobile brake disc and the preparation method thereof according to claim 2, characterized in that: In step 2, the powder required for the coating is prepared. First, the weight of each element powder is accurately weighed using an electronic balance with an accuracy of 0.001g. The weighed powder is mixed using a Wzm-10L mixer. The mixer speed is 250rad / min and the mixing time is 3 hours. The mixed powder is dried in a drying oven for 2 hours to prevent the powder from being oxidized.

6. The laser cladding high-hardness and wear-resistant coating on the surface of an automobile brake disc and the preparation method thereof according to claim 3, characterized in that: The process parameters of laser cladding technology in step three are: laser power 700-1000W, powder feeding rate 10-13g / min, scanning speed 5-10mm / s, spot diameter 2-4mm, overlap rate 30-45%, and the laser cladding protective gas is argon with a purity of ≥99.9%, and the protective gas flow rate is 10-15L / min.

Citation Information

Cited By

  • Preparation method for laser cladding of iron-based alloy wear-resistant coating on surface of automobile brake disc

    CN120666330A