Black phospho / WS2 composite defect material, preparation method and hydrogen evolution material
By constructing defective structures on black phosphorus and WS2 materials, and preparing low-particle composite nanosheets by segmented ultrasound and ball milling methods, the problem of insufficient activity of existing catalysts was solved, and the electrocatalytic performance and stability of the catalyst were significantly improved.
Patent Information
- Application Number
- CN202411295138.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-15
- Publication Date
- 2024-11-29
AI Technical Summary
The existing non-precious metal HER catalysts have insufficient catalytic activity during hydrogen electrolysis, which limits their widespread use in industrial applications, especially compared with Pt/C catalysts, which have a performance gap.
By constructing defective structures on black phosphorus and WS2 materials, low-particle black phosphorus/WS2 composite nanosheets were prepared by segmented ultrasonic process and ball milling, and the electronic structure was adjusted to enhance catalytic activity.
The electrocatalytic activity and stability of the catalyst are significantly improved, and the overpotential decreases at the same current density, and the stability of the catalyst is basically without attenuation after 5000 cycles.
Smart Images

Figure CN119040949A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical engineering and relates to a novel preparation method of a black phosphorus / WS2 composite defect material and testing of its efficient hydrogen evolution performance. Background Art
[0002] As a renewable energy with high energy density, hydrogen has received widespread attention for the use of green electricity to electrolyze water to produce green hydrogen with the continuous development of renewable energy such as photovoltaic power generation and wind power in recent years. It has been demonstrated and applied in hydrogen fuel vehicles, energy storage, petrochemicals, steel smelting and other fields, and has received strong support from relevant national policies.
[0003] In the process of producing hydrogen by electrolysis of water, lower overpotential means lower energy consumption, and this process often occurs on efficient hydrogen evolution catalysts. The currently mainstream Pt-based catalysts have high loading and high price, which limits the industrial application of HER catalysts. Therefore, high performance, low cost and easy preparation have become the mainstream research direction for the development of HER catalysts in the future.
[0004] Among the many studies on non-precious metal HER catalysts, transition metal sulfides have attracted much attention in the field of hydrogen evolution catalysis due to their low cost and high catalytic activity. However, compared with commercial Pt / C catalysts, they still have the problem of insufficient catalytic activity. By constructing atomic defects on the surface of transition metal sulfides, adjusting the electronic structure and heteroatom doping, their hydrogen evolution catalytic performance can be effectively improved. Black phosphorus itself has the characteristics of a two-dimensional single semiconductor with a direct band gap, which has broad application prospects in adjusting the electronic structure and optimizing the electrocatalytic activity. Studies have shown that black phosphorus can achieve bonding with Pt within a few minutes at room temperature to form a composite material, adjust the electronic structure, and increase its hydrogen evolution efficiency by 3.5 times. Summary of the invention
[0005] Based on the difficulties of the prior art, the present invention provides a black phosphorus / WS2 composite defect material. The present invention also provides a novel preparation method of the black phosphorus / WS2 defect material; the present invention also provides a method for testing the efficient hydrogen evolution performance of the black phosphorus / WS2 defect material.
[0006] The purpose of the present invention is achieved by the following technical means: On the one hand, the present invention provides a novel preparation method of black phosphorus nanosheet material and black phosphorus / WS2 defective nanosheet. In this method, it is verified that after the black phosphorus micropowder (D90≈10μm) is pre-treated by bubbling ultrasound, it is filtered out by a filter membrane, and then dispersed in a new dispersion liquid, bubbled and ultrasonicated, and the upper clear liquid is taken after centrifugation to obtain black phosphorus nanosheets with extremely low particle size. This method achieves a reduction of about 50 times in the particle size of black phosphorus under the same ultrasonic time, and the effect is significant. WS2 and black phosphorus micropowder are first pre-treated by ultrasonication to obtain smaller-sized flakes, filtered out by a filter membrane, and then dispersed again for bubbling ultrasound. The supernatant is taken by centrifugation and washed to obtain a BP / WS2 nanosheet composite material; the BP / WS2 nanosheet composite material is ball-milled to obtain a BP / WS2 composite defect material.
[0007] On the other hand, the present invention provides an application of black phosphorus / WS2 defect material as a hydrogen evolution material, and also provides a method for testing the performance of efficient hydrogen evolution. Prepare a mixed solution of water (130 μL), ethanol (130 μL) and Nafion solution (40 μL), disperse 3 mg of catalyst sample and 3 mg of acetylene black in the mixed solution, and mix them evenly by ultrasonic for 1 h. Take 100 μL of the above dispersion and evenly coat it on a 1 cm 2 The carbon fiber paper was placed on it, dried at room temperature, and then placed in a 60℃ vacuum drying oven for 6 hours for later use.
[0008] The carbon fiber paper loaded with catalyst was clamped on the electrode clamp as the working electrode, the graphite rod was used as the auxiliary electrode, the Ag / AgCl electrode of saturated KCl solution was used as the reference electrode, and 0.5 mol.L -1 The electrochemical performance test was carried out with H2SO4 solution as the electrolyte. The catalyst activity test was carried out with 5mv.s -1 The linear scanning curve obtained by the scanning rate was taken as the standard. The catalyst stability test was carried out after 5000 cycles at a current density of 50 mA.cm 2 The overpotential decay is measured below.
[0009] Compared with the prior art, the present invention has the following technical advantages: 1. The present invention provides a preparation process for low-particle-size nanosheets. Black phosphorus / WS2 micropowder is treated by a segmented bubbling ultrasonic process. After the first ultrasonic pretreatment, filtration and re-dispersion, and continuous bubbling operation, the front-end large-particle-size micropowder is rapidly peeled off to a two-dimensional layered structure and the rear-end two-dimensional layered material is nanosized. The prepared nanosheet dispersion has a high concentration (>100 mg / ml) and a low particle size (<500 nm).
[0010] 2. In the black phosphorus / WS2 composite defect material provided by the present invention, black phosphorus and tungsten sulfide material are subjected to segmented ultrasound to produce nano-scale doped composites, so that the ability of black phosphorus to adjust the electronic structure can be fully exerted, and by subsequently controlling relevant parameters in the ball milling process, a surface multi-defect structure is manufactured, thereby achieving the effect of improving the electrocatalytic performance of the composite defect material.
[0011] 3. The electrocatalytic activity of the black phosphorus / WS2 composite defect material prepared by co-ultrasonication and ball milling is several times higher than that of the conventional WS2 defect material, 50mA.cm 2 At a current density of 1.5 MW, the overpotential of BP / WS2 nanosheets is only 150 mV, which is much lower than that of defective WS2 nanosheets. At the same current density, the overpotential of BP / WS2 nanosheets is only one-third of that of WS2 nanosheets. After 5000 cycles, the stability of the catalyst shows that the LSV polarization curve changes little from the initial curve, and the electrochemical performance has basically no attenuation.
[0012] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 Black phosphorus nanosheet particle size test data of Example 2.
[0014] Figure 2 The LSV curves of the catalysts of Examples 3-8 are shown in FIG.
[0015] Figure 3 This is the CV curve picture of the catalyst of Example 5. Specific implementation methods In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0017] A method for preparing a black phosphorus / WS2 defect material comprises the following steps: Step 1: Disperse black phosphorus powder and tungsten sulfide powder in ethanol solution, perform bubbling and ultrasonic treatment in the first stage, filter, disperse again, perform bubbling and ultrasonic treatment in the second stage, centrifuge and separate the supernatant to obtain solution A; Step 2: Filter the solution A obtained in step 1, wash with water and centrifuge three times, then freeze-dry and collect the sample, which is recorded as sample A; Step 3: Take sample A obtained in step 2 and add it into a zirconia jar, evacuate the air, and fill it with inert gas; put it into a high-energy ball mill for ball milling to obtain a black phosphorus / WS2 composite defect material, which is recorded as sample B.
[0018] The power of the ultrasonic cell disruptor is 500-1000W, the ultrasonic temperature is controlled at 10-20°C, the magnetic stirring speed is 100-300r / min, and the amplitude is 10-70μm.
[0019] Under this power condition, nanoscale exfoliation of black phosphorus and tungsten sulfide powders was achieved, and the unique physical and chemical properties of black phosphorus were used to adjust the electronic structure of tungsten sulfide at the nanoscale to enhance the electrocatalytic activity.
[0020] Through the segmented ultrasonic process, nano-scale exfoliation of black phosphorus and tungsten sulfide materials is achieved, and the doping effect is better.
[0021] In step 1: bubbling ultrasound uses nitrogen bubbling, and the flow rate is controlled at 100-400 ml / min.
[0022] In step 1: the first stage of bubbling ultrasound time is 3-6 hours, and the second stage of bubbling ultrasound time is 12-24 hours.
[0023] On the one hand, nitrogen bubbling ultrasound can avoid the rapid oxidation of black phosphorus nanosheets obtained by ultrasound in an oxygen-containing environment. On the other hand, the cavitation effect generated by nitrogen bubbling can be used to enhance the ultrasonic stripping effect.
[0024] In step 1: the centrifugal speed is 1000-2000r·min -1 , centrifugation time 15-30min.
[0025] In step 1: the mass ratio of tungsten sulfide to black phosphorus is 1:0.1-0.3.
[0026] The appropriate amount of black phosphorus doping can effectively adjust the surface electronic structure of tungsten sulfide. Excessive black phosphorus can easily cover the surface defects of tungsten sulfide during the ball milling process of the back-end materials, and the electrocatalytic performance cannot be effectively improved.
[0027] In step three: the inert gas is argon; the ball mill uses 3.8-10 mm zirconium beads, a ball-to-material ratio of 2-5:1, a rotation speed of 500-1000 r / min, a ball mill power of 200-400 W, a ball mill time of 1-3 h, and a ball mill pressure of 20-50 bar.
[0028] Example 1 This embodiment provides an ultrasonic preparation method of ethanol phase black phosphorus nanosheets, comprising the following steps: Step 1: Disperse 2 g of black phosphorus powder in 100 ml of ethanol and use a 720W ultrasonic cell disruptor to ultrasonicate for 30 h to obtain dispersion A.
[0029] Step 2: Take 20ml of dispersion A and centrifuge at 1000r.min -1 After centrifugation for 15 min, the supernatant was collected and the sample was recorded as BP-1. The particle size test results are shown in Table 1.
[0030] Step 3: Take the dispersion A obtained in step 1 and centrifuge at 1000 r.min -1 The black phosphorus nanosheets were washed with water and centrifuged three times, and the samples were collected by freeze drying.
[0031] Example 2 This embodiment provides a segmented bubbling ultrasonic preparation method for ethanol phase black phosphorus nanosheets, comprising the following steps: Step 1: Disperse 2 g of black phosphorus powder in 100 ml of ethanol, use a 720 W ultrasonic cell disruptor to bubble and sonicate for 6 h, with a bubbling flow rate of 200 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 24 h to obtain dispersion A.
[0032] Step 2: Take 20ml of dispersion A and centrifuge at 1000r.min -1 Centrifuge for 15 minutes, take the supernatant, and record the sample as BP-2. The particle size test results are shown in Table 1. Figure 1 .
[0033] Step 3: Take the dispersion A obtained in step 1 and centrifuge at 1000 r.min -1 The black phosphorus nanosheets were washed with water and centrifuged three times, and the samples were collected by freeze drying.
[0034] Table 1 Black phosphorus nanosheet wet particle size data
[0035] Example 3 This embodiment provides a method for preparing WS2 defective nanosheets, comprising the following steps: Step 1: Disperse 2 g of tungsten sulfide powder in 100 ml of ethanol, use a 720W ultrasonic cell disruptor to bubble and sonicate for 6 h, with a bubbling flow rate of 200 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 24 h with a bubbling flow rate of 200 ml / min to obtain dispersion A.
[0036] Step 2: Take the dispersion A obtained in step 1 and centrifuge at 1000 r.min -1 After centrifugation for 15 min, the supernatant was removed to obtain WS2 nanosheets. The obtained WS2 nanosheets were washed with water and centrifuged three times, and the samples were collected by freeze drying.
[0037] Step 3: Take 100 mg of the tungsten sulfide nanosheets obtained in step 2 and add them to a zirconium oxide jar, remove the air, and fill it with argon. Put it into a 200W high-energy ball mill with 3.5mm zirconium beads, a ball-to-material ratio of 3:1, a speed of 500r / min, ball milling for 2h, and a pressure of 20bar to obtain defective WS2 nanosheets (denoted as WS2).
[0038] Step 4: Disperse 3 mg of nanosheets obtained in step 3 and 3 mg of acetylene black in a mixed solution (water, ethanol, Nafion) and mix them evenly by ultrasonic for 1 hour. Take 100 μL of the above dispersion and spread it evenly on a 1 cm 2 The catalyst was placed on carbon fiber paper, dried at room temperature, and then placed in a 60°C vacuum drying oven for 6 hours for use. The LSV curve of the catalyst electrocatalytic performance test is shown in Figure 2.
[0039] Example 4 This embodiment provides a method for preparing a BP / WS2 composite defect material, comprising the following steps: Step 1: Disperse 2 g of tungsten sulfide powder in 100 ml of ethanol, use a 720W ultrasonic cell disruptor to bubble and sonicate for 6 h, with a bubbling flow rate of 200 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 24 h with a bubbling flow rate of 200 ml / min to obtain dispersion A.
[0040] Step 2: Take the dispersion A obtained in step 1 and centrifuge at 1000 r.min -1 After centrifugation for 15 min, the supernatant was removed to obtain WS2 nanosheets. The obtained WS2 nanosheets were washed with water and centrifuged three times, and the samples were collected by freeze drying and recorded as sample A.
[0041] Step 3: Disperse 2 g of black phosphorus powder in 100 ml of ethanol, use a 720 W ultrasonic cell disruptor to bubble and sonicate for 6 h at a bubbling flow rate of 200 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol at a bubbling flow rate of 200 ml / min for 24 h to obtain dispersion B.
[0042] Step 4: Take the dispersion B obtained in step 3 and centrifuge at 1000r.min -1 After centrifugation for 15 minutes, the supernatant was removed to obtain black phosphorus nanosheets. The obtained black phosphorus nanosheets were washed with water and centrifuged three times, and freeze-dried to collect the sample, which was recorded as sample B.
[0043] Step 5: Take 90 mg of sample A and 10 mg of sample B, totaling 100 mg, and add them into a zirconium oxide can, evacuate the air, and fill it with argon. Put it into a 200W high-energy ball mill with 3.5mm zirconium beads, a ball-to-material ratio of 3:1, a speed of 500r / min, ball milling for 2h, and a pressure of 20bar to obtain BP / WS2 defective material (referred to as BP / WS2-1).
[0044] Step 6: Disperse 3 mg of BP / WS2 defective material obtained in step 5 and 3 mg of acetylene black in a mixed solution (water, ethanol, Nafion) and mix them evenly by ultrasonic for 1 hour. Take 100 μL of the above dispersion and evenly apply it on a 1 cm 2 The catalyst was placed on carbon fiber paper, dried at room temperature, and then placed in a 60°C vacuum drying oven for 6 hours for use. The LSV curve of the catalyst electrocatalytic performance test is shown in Figure 2.
[0045] Example 5 This embodiment provides a method for preparing a BP / WS2 composite defect material, comprising the following steps: Step 1: Disperse 1.8 g of tungsten sulfide powder and 0.2 g of black phosphorus powder in 100 ml of ethanol, use a 720 W ultrasonic cell disruptor to bubble and sonicate for 6 h at a bubbling flow rate of 200 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 24 h at a bubbling flow rate of 200 ml / min to obtain dispersion A.
[0046] Step 2: Take the dispersion A obtained in step 1 and centrifuge at 1000 r.min -1 Centrifuge for 15 minutes, remove the supernatant, and obtain the composite nanosheets. Wash the obtained composite nanosheets with water and centrifuge for three times, and freeze-dry to collect the samples.
[0047] Step 3: Take 100 mg of the sample obtained in step 2 and add it to a zirconium oxide jar, evacuate the air, and fill it with argon. Put it into a 200W high-energy ball mill with 3.5mm zirconium beads, a ball-to-material ratio of 3:1, a speed of 500r / min, ball milling for 2h, and a pressure of 20bar to obtain BP / WS2 defective material (referred to as BP / WS2-2).
[0048] Step 4: Disperse 3 mg of BP / WS2 defective material obtained in step 3 and 3 mg of acetylene black in a mixed solution (water, ethanol, Nafion) and mix them evenly by ultrasonic for 1 hour. Take 100 μL of the above dispersion and evenly coat it on a 1 cm 2 The catalyst was placed on carbon fiber paper, dried at room temperature, and then placed in a 60°C vacuum drying oven for 6 hours for use. The LSV curve of the catalyst electrocatalytic performance test is shown in Figure 2, and the LSV test curve of the catalyst stability test after 5000 cycles is shown in Figure 3.
[0049] Example 6 This embodiment provides a method for preparing a BP / WS2 composite defect material, comprising the following steps: Step 1: Disperse 1.8 g of tungsten sulfide powder and 0.2 g of black phosphorus powder in 100 ml of ethanol, use a 500 W ultrasonic cell disruptor to bubble and sonicate for 3 h at a bubbling flow rate of 100 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 12 h at a bubbling flow rate of 100 ml / min to obtain dispersion A.
[0050] Step 2: Take the dispersion A obtained in step 1 and centrifuge at 500 r.min -1 The composite nanosheets were washed with water and centrifuged three times, and the samples were collected by freeze drying.
[0051] Step 3: Take 100 mg of the sample obtained in step 2 and add it to a zirconium oxide jar, remove the air, and fill it with argon. Put it into a 200W high-energy ball mill, select 5mm zirconium beads, ball-to-material ratio 2:1, speed 200r / min, ball milling power 100W, ball milling for 1h, pressure 10bar, and obtain BP / WS2 defect material (referred to as BP / WS2-3).
[0052] Step 4: Disperse 3 mg of BP / WS2 defective material obtained in step 3 and 3 mg of acetylene black in a mixed solution (water, ethanol, Nafion) and mix them evenly by ultrasonic for 1 hour. Take 100 μL of the above dispersion and evenly coat it on a 1 cm 2 The catalyst was placed on carbon fiber paper, dried at room temperature, and then placed in a 60°C vacuum drying oven for 6 hours for use. The LSV curve of the catalyst electrocatalytic performance test is shown in Figure 2.
[0053] Example 7 This embodiment provides a method for preparing a BP / WS2 composite defect material, comprising the following steps: Step 1: Disperse 1.8 g of tungsten sulfide powder and 0.2 g of black phosphorus powder in 100 ml of ethanol, use a 1000 W ultrasonic cell disruptor to bubble and sonicate for 12 h at a bubbling flow rate of 400 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 36 h at a bubbling flow rate of 400 ml / min to obtain dispersion A.
[0054] Step 2: Take the dispersion A obtained in step 1 and centrifuge at 2000r.min -1 The composite nanosheets were washed with water and centrifuged three times, and the samples were collected by freeze drying.
[0055] Step 3: Take 100 mg of the sample obtained in step 2 and add it to a zirconium oxide jar, evacuate the air, and fill it with argon. Put it into a 200W high-energy ball mill, select 10mm zirconium beads, ball-to-material ratio 5:1, speed 500r / min, ball milling power 400W, ball milling for 3h, pressure 30bar, and obtain BP / WS2 defect material (referred to as BP / WS2-4).
[0056] Step 4: Disperse 3 mg of BP / WS2 defective material obtained in step 3 and 3 mg of acetylene black in a mixed solution (water, ethanol, Nafion) and mix them evenly by ultrasonic for 1 hour. Take 100 μL of the above dispersion and evenly coat it on a 1 cm 2 The catalyst was placed on carbon fiber paper, dried at room temperature, and then placed in a 60°C vacuum drying oven for 6 hours for use. The LSV curve of the catalyst electrocatalytic performance test is shown in Figure 2.
[0057] Example 8 This embodiment provides a method for preparing a BP / WS2 composite defect material, comprising the following steps: Step 1: Disperse 1.6 g of tungsten sulfide powder and 0.4 g of black phosphorus powder in 100 ml of ethanol, use a 720 W ultrasonic cell disruptor to bubble and sonicate for 6 h at a bubbling flow rate of 200 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 24 h at a bubbling flow rate of 200 ml / min to obtain dispersion A.
[0058] Step 2: Take the dispersion A obtained in step 1 and centrifuge at 1000 r.min -1 Centrifuge for 15 minutes, remove the supernatant, and obtain the composite nanosheets. Wash the obtained composite nanosheets with water and centrifuge for three times, and freeze-dry to collect the samples.
[0059] Step 3: Take 100 mg of the sample obtained in step 2 and add it to a zirconium oxide jar, evacuate the air, and fill it with argon. Put it into a 200W high-energy ball mill with 3.5mm zirconium beads, a ball-to-material ratio of 3:1, a speed of 500r / min, ball milling for 2h, and a pressure of 20bar to obtain BP / WS2 defective material (referred to as BP / WS2-5).
[0060] Step 4: Disperse 3 mg of BP / WS2 composite defect material obtained in step 3 and 3 mg of acetylene black in a mixed solution (water, ethanol, Nafion) and mix them evenly by ultrasonic for 1 hour. Take 100 μL of the above dispersion and evenly coat it on a 1 cm 2 The catalyst was placed on carbon fiber paper, dried at room temperature, and then placed in a 60°C vacuum drying oven for 6 hours for use. The LSV of the catalyst electrocatalytic performance test is shown in Figure 2.
[0061] Example 9 This embodiment provides a method for preparing a BP / WS2 composite defect material, comprising the following steps: Step 1: Disperse 1.8 g of tungsten sulfide powder and 0.2 g of black phosphorus powder in 100 ml of ethanol, use a 300 W ultrasonic cell disruptor to bubble and sonicate for 6 h at a bubbling flow rate of 200 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 24 h at a bubbling flow rate of 200 ml / min to obtain dispersion A.
[0062] Step 2: Take the dispersion A obtained in step 1 and centrifuge at 1000 r.min -1 Centrifuge for 15 minutes, remove the supernatant, and obtain the composite nanosheets. Wash the obtained composite nanosheets with water and centrifuge for three times, and freeze-dry to collect the samples.
[0063] Step 3: Take 100 mg of the sample obtained in step 2 and add it to a zirconium oxide jar, evacuate the air, and fill it with argon. Put it into a 200W high-energy ball mill with 3.5mm zirconium beads, a ball-to-material ratio of 3:1, a speed of 500r / min, ball milling for 2h, and a pressure of 20bar to obtain BP / WS2 defective material (referred to as BP / WS2-6).
[0064] Step 4: Disperse 3 mg of BP / WS2 defective material obtained in step 3 and 3 mg of acetylene black in a mixed solution (water, ethanol, Nafion) and mix them evenly by ultrasonic for 1 hour. Take 100 μL of the above dispersion and evenly coat it on a 1 cm 2 The catalyst was placed on carbon fiber paper, dried at room temperature, and then placed in a 60°C vacuum drying oven for 6 hours for use. Figure 2 shows the LSV of the catalyst electrocatalytic performance test.
[0065] Example 10 This embodiment provides a method for preparing a BP / WS2 composite defect material, comprising the following steps: Step 1: Disperse 1.8 g of tungsten sulfide powder and 0.2 g of black phosphorus powder in 100 ml of ethanol, use a 720 W ultrasonic cell disruptor to bubble and sonicate for 1 h, the bubbling flow rate is 200 ml / min, filter with a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 24 h at a bubbling flow rate of 200 ml / min to obtain dispersion A.
[0066] Step 2: Take the dispersion A obtained in step 1 and centrifuge at 1000 r.min -1 Centrifuge for 15 minutes, remove the supernatant, and obtain the composite nanosheets. Wash the obtained composite nanosheets with water and centrifuge for three times, and freeze-dry to collect the samples.
[0067] Step 3: Take 100 mg of the sample obtained in step 2 and add it to a zirconium oxide jar, evacuate the air, and fill it with argon. Put it into a 200W high-energy ball mill with 3.5mm zirconium beads, a ball-to-material ratio of 3:1, a speed of 500r / min, ball milling for 2h, and a pressure of 20bar to obtain BP / WS2 defective material (referred to as BP / WS2-7).
[0068] Step 4: Disperse 3 mg of BP / WS2 defective material obtained in step 3 and 3 mg of acetylene black in a mixed solution (water, ethanol, Nafion) and mix them evenly by ultrasonic for 1 hour. Take 100 μL of the above dispersion and evenly coat it on a 1 cm 2 The catalyst was placed on carbon fiber paper, dried at room temperature, and then placed in a 60°C vacuum drying oven for 6 hours for use. Figure 2 shows the LSV of the catalyst electrocatalytic performance test.
[0069] Embodiment 11 This embodiment provides a method for preparing a BP / WS2 composite defect material, comprising the following steps: Step 1: Disperse 1.8 g of tungsten sulfide powder and 0.2 g of black phosphorus powder in 100 ml of ethanol, use a 720 W ultrasonic cell disruptor to bubble and sonicate for 6 h at a bubbling flow rate of 30 ml / min, filter using a filter membrane, collect the filtrate, and then disperse it in 100 ml of ethanol, bubble and sonicate for 24 h at a bubbling flow rate of 30 ml / min to obtain dispersion A.
[0070] Step 2: Take the dispersion A obtained in step 1 and centrifuge at 1000 r.min -1 Centrifuge for 15 minutes, remove the supernatant, and obtain the composite nanosheets. Wash the obtained composite nanosheets with water and centrifuge for three times, and freeze-dry to collect the samples.
[0071] Step 3: Take 100 mg of the sample obtained in step 2 and add it to a zirconium oxide jar, evacuate the air, and fill it with argon. Put it into a 200W high-energy ball mill with 3.5mm zirconium beads, a ball-to-material ratio of 3:1, a speed of 500r / min, ball milling for 2h, and a pressure of 20bar to obtain BP / WS2 defective material (referred to as BP / WS2-8).
[0072] Step 4: Disperse 3 mg of BP / WS2 defective material obtained in step 3 and 3 mg of acetylene black in a mixed solution (water, ethanol, Nafion) and mix them evenly by ultrasonic for 1 hour. Take 100 μL of the above dispersion and evenly coat it on a 1 cm 2 The catalyst was placed on carbon fiber paper, dried at room temperature, and then placed in a 60°C vacuum drying oven for 6 hours for use. Figure 2 shows the LSV of the catalyst electrocatalytic performance test.
[0073] The segmented ultrasonic process of the present invention can achieve full stripping of two-dimensional materials black phosphorus and tungsten sulfide. The particle size of black phosphorus micropowder (D90≈10μm) can be reduced to hundreds of nanometers after segmented ultrasonic treatment in the ethanol phase, which is nearly 50 times lower. The black phosphorus nanosheets have high dispersibility. There is basically no sample loss in the preparation process, and it can be used to prepare high-concentration (>20mg / ml) nanosheet dispersions. The low-particle size BP / WS2 composite defect material prepared by the segmented ultrasonic process has high electrochemical activity. At the same current density, the overpotential of the BP / WS2 catalyst is only 1 / 3 of that of the defective WS2 catalyst, and the activity is significantly improved.
[0074] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a black phosphorus / WS2 defect material, characterized in that: The following steps are involved: Step 1: Disperse black phosphorus powder and tungsten sulfide powder in ethanol solution, perform bubbling and ultrasonic treatment in the first stage, filter, disperse again, perform bubbling and ultrasonic treatment in the second stage, centrifuge and separate the supernatant to obtain solution A; Step 2: Filter the solution A obtained in step 1, wash with water and centrifuge three times, then freeze-dry and collect the sample, which is recorded as sample A; Step 3: Take sample A obtained in step 2 and add it into a zirconia jar, evacuate the air, and fill it with inert gas; put it into a high-energy ball mill for ball milling to obtain a black phosphorus / WS2 composite defect material, which is recorded as sample B.
2. The preparation method according to claim 1, characterized in that In step 1: the power of the ultrasonic cell disruptor is 500-1000W, the ultrasonic temperature is controlled at 10-20°C, the magnetic stirring speed is 100-300r / min, and the amplitude is 10-70μm.
3. The preparation method according to claim 1, characterized in that: In step 1: bubbling ultrasound uses nitrogen bubbling, and the flow rate is controlled at 100-400 ml / min.
4. The preparation method according to claim 1, characterized in that: In step 1: the first stage of bubbling ultrasound time is 3-6 hours, and the second stage of bubbling ultrasound time is 12-24 hours.
5. The preparation method according to claim 1, characterized in that: In step 1: the centrifugal speed is 1000-2000r·min -1 , centrifugation time 15-30min.
6. The preparation method according to claim 1, characterized in that: In step 1: add tungsten sulfide and black phosphorus in a mass ratio of 1:0.1-0.
3.
7. The preparation method according to claim 1, characterized in that: In step three: the inert gas is argon; the ball mill uses 3.8-10 mm zirconium beads, a ball-to-material ratio of 2-5:1, a rotation speed of 500-1000 r / min, a ball mill power of 200-400 W, a ball mill time of 1-3 h, and a ball mill pressure of 20-50 bar.
8. A black phosphorus / WS2 composite defect material, characterized in that: Including black phosphorus / WS2 defect material prepared by the preparation method described in any one of claims 1-7.
9. A hydrogen evolution material, characterized in that: Including the black phosphorus / WS2 composite defect material as described in claim 8.