Multistage structure transition metal modified carbon nanofiber and preparation method thereof

By increasing the doping concentration and control structure in ZIFs materials, multi-stage structural transition metal modified carbon nanofibers were prepared, which solved the problems of low doping concentration and agglomeration, and achieved high-efficiency energy conversion and improved device integration.

CN119041055APending Publication Date: 2024-11-29HENAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411168638.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the low doping concentration and agglomeration of ZIFs materials lead to failure of nano-size effect, making it difficult to prepare carbon nanofibers modified with multi-stage structural transition metals.

Method used

The transition metal modified polymer nanofiber precursor is prepared by using high-carbon yield polymers, easily dissolved polymers and metal salts in organic solvents, and the transition metal modified polymer nanofiber precursors are soaked in organic ligand solution to form a multi-stage structure. Then, carbonization is heated at high temperature in a tube furnace to obtain multi-stage structural transition metal modified carbon nanofibers.

Benefits of technology

Improves the metal ion doping ratio and material stability, ensures the continuous structure and efficient energy conversion performance of the fiber, enhances device integration, and limits the fiber size by controlling the hole and capsulating agent size, achieving efficient Energy conversion and wide application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041055A_ABST
    Figure CN119041055A_ABST
Patent Text Reader

Abstract

The invention provides a multilevel structure transition metal modified carbon nanofiber and a preparation method thereof, belongs to the technical field of nanofiber materials, and aims to solve the technical problems that a ZIFs material is low in doping concentration, and agglomeration and morphology are not easy to control. The preparation method comprises the following steps: (1) mixing and dissolving a high-carbon-yield polymer, a soluble polymer, a metal salt and a solvent to obtain a spinning solution; (2) spinning the spinning solution by adopting a spinning process to obtain a transition metal modified polymer nanofiber precursor; (3) soaking the transition metal modified polymer nanofiber precursor in a solution containing an organic ligand to obtain a multilevel structure transition metal modified polymer nanofiber; and (4) calcining and carbonizing the multi-stage structure transition metal modified polymer nanofiber to obtain the multi-stage structure transition metal modified carbon nanofiber. By adjusting the ratio of the solution to the polymer, the dissolving speed and concentration of the metal salt in the mixed solution can be controlled, and the size of the metal organic framework is adjustable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanofiber materials, and in particular relates to a multi-level structure transition metal modified carbon nanofiber and a preparation method thereof. Background Art

[0002] As the global population increases and non-renewable resources decrease, energy crisis, environmental crisis and global warming have become key issues restricting the development of human society. At present, carbon dioxide reduction, nitrogen fixation and ammonia synthesis, water decomposition and hydrogen production, solar and biomass power generation, and organic pollutant degradation are key industries to solve the above problems. The reaction processes of the above industries require efficient functional materials to reduce reaction barriers, improve reaction efficiency and reduce environmental pollution. Therefore, the development of efficient and stable functional materials is the focus of current energy, environment and manufacturing fields.

[0003] Nanomaterials have become the key to the preparation of efficient functional materials due to their high specific surface area, size effect, excellent mechanical properties and customizability, showing unique physical and chemical properties. Among them, metal organic frameworks are a type of porous structure materials formed by metal ion clusters and organic ligands through coordination bonds, which have the characteristics of high specific surface area, adjustable pore size and multifunctional functional groups. Dimethylimidazole, as a commonly used nitrogen-containing organic ligand, has strong coordination ability, good thermal stability and chemical stability, which provides a basis for the preparation of nitrogen-doped metal organic framework materials. The metal organic frameworks (Zeolitic Imidazolate Frameworks, ZIFs) prepared by dimethylimidazole have become one of the core materials for reducing energy barriers and environmental pollution. However, the central metal cation of ZIFs is required to be divalent and have a tetrahedral configuration, such as Co2 + 、Zn 2+ This requirement limits its development. It has been proven that doping with iron, nickel and manganese ions is an effective way to regulate the surface charge distribution and active centers of atoms, but they do not satisfy the positive divalent or tetrahedral configuration, making it difficult to dope them into ZIFs.

[0004] At present, iron ions are often doped into ZIFs through hydrothermal method, adsorption method and conversion method. The hydrothermal method is to add iron and other doping ions to a divalent metal precursor solution and react with a dimethyl imidazole solution to obtain iron ion doped ZIFs. Some iron ions can be doped, but there are problems of low iron ion concentration and reduced ZIFs yield. The adsorption method is to physically mix the synthesized ZIFs with iron ion salts, or the synthesized ZIFs are etched with weak acid or weak base and then the iron ion salts are adsorbed on the ZIFs. This method has the problems of low iron ion concentration and no chemical bond between iron and cobalt ions. The conversion method refers to the reaction of the synthesized ZIFs with the doping ion solution to form a new material. For example, cobalt-based ZIFs are placed in a nickel salt solution for hydrothermal reaction to form CoNi hydroxide on the surface. This method has the problems of low doping ion concentration and ZIFs structural destruction. On the other hand, the doped ZIFs currently prepared are powder materials, and the agglomeration driven by van der Waals forces leads to the failure of the nanosize effect. Therefore, it is imperative to use an optimized method to increase the iron plasma doping concentration to prepare multi-level structured transition metal-modified carbon nanofibers.

[0005] Patent Publication No. CN 115810765 A discloses a carbon nanofiber catalyst and its preparation method and application. The preparation method comprises the following steps: (1) preparing ZnM-ZIF powder by coprecipitation of zinc salt and transition metal salt; (2) mixing a polymer source, an organic solvent and the ZnM-ZIF powder obtained in step (1), stirring evenly to obtain a spinning solution; (3) preparing a fiber precursor by electrospinning the spinning solution obtained in step (2); (4) heat-treating the fiber precursor obtained in step (3) to obtain a carbon nanofiber catalyst. Patent Publication No. CN 114695888A discloses a carbon nanofiber composite material and its preparation method and application. Carbon particles derived from ZIF-8 nanoparticles are connected in series by carbon nanofibers through electrospinning, in-situ growth and high-temperature carbonization to prepare a carbon nanofiber composite material modified with porous carbon polyhedrons. The above two patents prepare ZIFs modified carbon fiber materials by doping and in-situ synthesis respectively. However, there are problems such as low ZnM-ZIF powder addition and easy agglomeration in doping, and there is a problem of difficult control of morphology in in-situ synthesis. Summary of the invention

[0006] In view of the technical problems of low doping concentration, agglomeration and difficult to control morphology of ZIFs materials, the present invention proposes a multi-level structure transition metal modified carbon nanofiber and a preparation method thereof, which solves the problems of low doping concentration and agglomeration of existing ZIFs materials and improves energy conversion efficiency and device integration.

[0007] In order to achieve the above object, the technical solution of the present invention is achieved as follows:

[0008] A multi-level structure transition metal modified carbon nanofiber, the preparation method comprises the following steps:

[0009] Step 1, mixing a high carbon yield polymer, a soluble polymer, a metal salt and an organic solvent, heating and stirring to obtain a spinning solution;

[0010] Step 2, spinning by a spinning process to obtain a transition metal modified polymer nanofiber precursor;

[0011] Step 3, soaking the transition metal modified polymer nanofiber precursor in a solution containing an organic ligand, generating a large number of pores inside the fiber, and growing a secondary structure on the fiber surface, thereby obtaining a multi-level structure transition metal modified polymer nanofiber;

[0012] Step 4, collecting and vacuum drying the multi-level transition metal modified polymer nanofibers;

[0013] Step 5, placing the dried multi-level transition metal modified polymer nanofibers into a tubular furnace, calcining in air for a short time, and then heating at a high temperature under a certain gas protection to obtain multi-level transition metal modified carbon nanofibers;

[0014] Preferably, in step 1, the concentration of the high carbon yield polymer is 5-10wt%, the concentration of the easily soluble polymer is 5-10wt%, and the concentration of the metal salt is 5-15wt%; the high carbon yield polymer is one or more of polyacrylonitrile with an average molecular weight of 100,000-200,000, polyvinyl pyrrolidone with a molecular weight of 1,000,000-1,300,000, or polyvinyl alcohol with a molecular weight of 85,000-124,000; the easily soluble polymer is one or more of polyvinyl pyrrolidone with a molecular weight less than 58,000 or / less than 30,000 molecular weight of polyvinyl alcohol; the metal salt is one or more of soluble salts such as sulfates, acetates, nitrates, acetylacetonates and chlorides; the organic solvent is one or more of dimethylacetamide, dimethylformamide and dimethyl sulfoxide; the solution heating and stirring temperature is 60-90°C, and the heating and stirring time is 5-48h.

[0015] Preferably, the spinning method in step 2 is one or more of wet spinning, dry spinning and electrospinning, the solution injection speed of wet spinning and dry spinning is 0.1-5ml / h, and the total traction ratio is 1-30; the solution injection speed of electrospinning is 0.1-3ml / h, the distance between the injector head and the receiver is 5-30cm, the receiver rotation speed is 0-3000r / min, the spinning temperature is 20-40℃, the humidity is 20-40%, and the voltage is 5-30kV.

[0016] Preferably, the organic ligand in step three is one or more of dimethylimidazole, terephthalic acid, trimesic acid, etc.; the solvent of the solution containing the organic ligand is one or more of methanol, ethanol and water; the concentration of the organic ligand is 0.1-0.8M; the immersion method is one or more of standing, stirring and ultrasound, and the time is 4-20h.

[0017] Preferably, the vacuum drying temperature in step 4 is 40-80°C, and the vacuum drying time is 4-48h.

[0018] Preferably, in step five, the air calcination heating rate is 1-10°C / min, the calcination temperature is 180-280°C, and the calcination time is 1-3h; the carbonization heating rate is 1-10°C / min, the carbonization temperature is 600-1800°C, and the carbonization time is 1-3h; and the cooling method is natural cooling with the furnace.

[0019] Beneficial effects of the present invention:

[0020] 1) High carbon yield polymers will not dissolve in the solution of organic ligands, which limits the movement and dissolution of metal ion clusters. The dissolution of soluble polymers causes metal ions to be exposed, and metal organic ligands coordinate with the exposed metal ions to form metal organic ligands. On the one hand, the restricted metal ions ensure the metal ion doping ratio, giving the material universal functionality and designability, which can be flexibly adjusted according to different needs. On the other hand, the restricted metal ions ensure that the synthesized metal organic framework is tightly attached to the nanofibers, the metal organic framework has a strong bonding force with the fibers, and the fiber material has a certain stability.

[0021] 2) As the soluble polymer dissolves, certain holes are generated inside the fiber. When the size of the metal organic framework grows to a size close to that of the hole, the confinement effect will limit its growth, thereby ensuring that the generated size is smaller than the size of the hole in the fiber. At the same time, the dissolved polymer acts as a capping agent to limit the size of the surface metal organic framework. The limiting effect of the hole size and the capping agent constitutes the unique confinement synthesis method of the present invention. By adjusting the ratio of the solution and the polymer, the dissolution rate and concentration of the metal salt in the mixed solution can be controlled, and the size of the metal organic framework is adjustable.

[0022] 3) The equipment required in this technical solution includes a magnetic stirrer, a vacuum drying oven, an electrospinning machine and a tubular furnace, etc., which are low-cost. The spinning process can realize large-scale and continuous preparation of nanofibers, and has the characteristics of stable process and high production efficiency. The technical solution is economical and universal.

[0023] 4) The prepared fiber material can be further subjected to physical and chemical treatments, such as vulcanization and nitridation, making it have a wide range of application potential. At the same time, the prepared fiber material can form a self-supporting membrane structure, avoiding the use of binders, thereby expanding its application field and having a high commercial application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 The present invention is a flow chart of a method for preparing multi-level structure transition metal carbon nanofibers;

[0026] Figure 2 This is a scanning electron microscope image of the hierarchical cobalt-iron metal carbon nanofiber obtained in Example 1;

[0027] Figure 3 This is a transmission electron microscope image of the hierarchical structured cobalt-iron metal carbon nanofiber obtained in Example 1;

[0028] Figure 4 This is a comparison chart of the oxygen evolution reaction and oxygen reduction reaction performance results of the hierarchical cobalt-iron metal carbon nanofibers obtained in Example 1 and commercial precious metals in 0.1M KOH solution. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] A multi-level transition metal modified carbon nanofiber, the process is as follows Figure 1 As shown, the specific preparation method comprises the following steps:

[0032] 10% by mass of cobalt nitrate and iron nitrate (mass ratio 1:1), 5% by mass of 150,000 molecular weight polyacrylonitrile, and 5% by mass of 8,000 molecular weight polyvinyl pyrrolidone were added to dimethylformamide, and the spinning solution was obtained by continuous stirring at 60°C for 48 hours.

[0033] The spinning solution was added to a 25 ml syringe and spun according to the parameters of injection speed of 1 ml / h, distance between syringe needle and receiver of 15 cm, receiver speed of 500 rpm, spinning temperature of 25°C, spinning humidity of 25%, and electrospinning voltage of 15 kV. After spinning, the fibers were collected and placed in a vacuum drying oven at 50°C for 12 hours to obtain cobalt-iron modified polymer nanofibers.

[0034] 2.4 g of dimethylimidazole was added to 80 ml of methanol solution, and stirred continuously at room temperature for 20 min in a magnetic stirrer at 500 rpm to obtain a clear solution. The fiber membrane cut into a certain size was placed in the solution, and gently shaken for 30 seconds every 10 minutes and the process lasted for 30 minutes, and finally stood at room temperature for 6 hours. The reacted fiber was placed in a methanol solution and washed three times continuously, and placed in a vacuum drying oven at 40°C for 48 hours to obtain a polymer nanofiber with a cobalt-iron-based metal organic framework on the surface.

[0035] The fiber was placed in a tubular furnace, heated to 280°C at a heating rate of 1°C / min in an air atmosphere and maintained for 2 hours, and then cooled to room temperature in the furnace. Then, the temperature was raised to 800°C at a heating rate of 1°C / min in a nitrogen atmosphere and maintained for 2 hours, and then cooled to room temperature in the furnace to obtain carbon nanofibers derived from a cobalt-iron-based metal organic framework.

[0036] Scanning electron microscopy images of carbon nanofibers derived from cobalt-iron metal organic frameworks Figure 2 As shown. After carbonization, the fiber maintains a continuous structure, the fiber surface is rough and the growth diameter is about 30nm CoFe ZIFs derivatives, 30nm CoFeZIFs derivatives are smaller than the CoFe ZIFs derivatives prepared by the hydrothermal method and in situ growth method. The transmission electron microscopy image of the carbon nanofibers derived from the cobalt-iron metal organic framework further proves that the fiber contains a large number of nanoparticles with a size of about 30nm. The small nanoparticles prove the advantage of the confined synthesis strategy ( Figure 3 To evaluate the fiber properties, the CoFe-MOF-derived carbon nanofibers were prepared by mixing with commercial noble metals Pt / C and RuO in 0.1 M KOH solution. 2 The oxygen reduction performance and oxygen evolution performance of Figure 4 The overpotential of oxygen evolution reaction of carbon nanofibers derived from cobalt-iron metal organic framework is 320mV, and the commercial noble metal RuO 2 The overpotential is 333 mV, which proves that the CoFe-based metal organic framework-derived carbon nanofibers have excellent oxygen evolution performance ( Figure 4a). The half-wave potential of oxygen reduction of the carbon nanofibers derived from the CoFe-based metal organic framework is 0.88 V, while the half-wave potential of commercial precious metal Pt / C is 0.863 V. The large half-wave potential proves that the carbon nanofibers derived from the CoFe-based metal organic framework have excellent oxygen reduction performance ( Figure 4 b). The excellent oxygen evolution and oxygen reduction properties of CoFe-based ZIFs are attributed to the fact that the small CoFe ZIFs derivatives provide more active sites, and the continuous fiber structure and interfiber pore structure are beneficial for electron and ion transport.

[0037] Example 2

[0038] A multi-level structure transition metal modified carbon nanofiber, the preparation method comprises the following steps:

[0039] 15% by mass of zinc nitrate and nickel nitrate (mass ratio 1:1), 5% by mass of 150,000 molecular weight polyacrylonitrile, and 5% by mass of 24,000 molecular weight polyvinyl pyrrolidone were added to dimethylacetamide, and the spinning solution was obtained by continuous stirring at 70°C for 12 hours.

[0040] The spinning solution was added to a 25 ml syringe and spun according to the parameters of injection speed of 0.1 ml / h, distance between syringe needle and receiver of 5 cm, receiver stationary, spinning temperature of 40°C, spinning humidity of 20%, and electrospinning voltage of 5 kV. After spinning, the fibers were collected and placed in a vacuum drying oven at 60°C for 12 hours to obtain nickel-zinc modified polymer nanofibers.

[0041] 2.4 g of dimethylimidazole was added to 80 ml of aqueous solution, and stirred continuously at room temperature for 20 min in a magnetic stirrer at 500 rpm to obtain a clear solution. The fiber membrane cut into a certain size was placed in the solution, ultrasonicated for 15 min, and finally allowed to stand at room temperature for 4 h. The reacted fiber was placed in a methanol solution and washed three times continuously, and placed in a vacuum drying oven at 60 ° C for 12 h to obtain a polymer nanofiber with a nickel-zinc-based metal organic framework on the surface.

[0042] The fiber was placed in a tubular furnace, heated to 180°C at a heating rate of 10°C / min in an air atmosphere and maintained for 3 hours, and then cooled to room temperature in the furnace. Then, the temperature was raised to 600°C at a heating rate of 10°C / min in an argon atmosphere and maintained for 1 hour, and then cooled to room temperature in the furnace to obtain a nickel-zinc-based metal organic framework-derived carbon nanofiber.

[0043] Example 3

[0044] A multi-level structure transition metal modified carbon nanofiber, the preparation method comprises the following steps:

[0045] 10% by mass of cobalt nitrate, ferric acetylacetonate, copper sulfate and manganese chloride (mass ratio 1:1:1:1), 8% by mass of 150,000 molecular weight polyacrylonitrile and 7% by mass of 10,000 molecular weight polyvinyl pyrrolidone were added to dimethyl sulfoxide solution, and the spinning solution was obtained by continuous stirring at 90°C for 5 hours.

[0046] The spinning solution was added to a 25 ml syringe and spun according to the parameters of injection speed of 3 ml / h, distance between syringe needle and receiver of 30 cm, receiver speed of 3000 rpm, spinning temperature of 20°C, spinning humidity of 40%, and electrospinning voltage of 30 kV. After spinning, the fibers were collected and placed in a vacuum drying oven at 50°C for 12 hours to obtain polymer nanofibers modified with cobalt, iron, copper and manganese.

[0047] 0.66 g of dimethylimidazole was added to 80 ml of ethanol solution, and stirred continuously at room temperature for 20 min in a magnetic stirrer at 500 rpm to obtain a clear solution. The fiber membrane cut into a certain size was placed in the solution and magnetic stirring was continued for 6 h. The reacted fiber was placed in the ethanol solution and washed three times continuously, and placed in a vacuum drying oven at 50 ° C for 12 h to obtain cobalt-iron-copper-manganese polymer nanofibers with metal organic frameworks on the surface.

[0048] The fiber was placed in a tubular furnace, heated to 250°C at a heating rate of 2°C / min in an air atmosphere and maintained for 2 hours, and then cooled to room temperature with the furnace. Then, the temperature was raised to 1800°C at a heating rate of 2°C / min in a nitrogen atmosphere and maintained for 3 hours, and then cooled to room temperature with the furnace to obtain carbon nanofibers derived from a cobalt-iron-copper-manganese-based metal organic framework.

[0049] Example 4

[0050] A multi-level structure transition metal modified carbon nanofiber, the preparation method comprises the following steps:

[0051] 5% by mass of manganese nitrate, iron nitrate and copper sulfate (mass ratio 1:1:1), 8% by mass of 150,000 molecular weight polyacrylonitrile and 5% by mass of 9,000 molecular weight polyvinyl alcohol were added to dimethylacetamide, and the spinning solution was obtained by continuous stirring at 60°C for 12 hours.

[0052] The spinning solution was added to a 25 ml syringe and spun according to the dry spinning parameters of injection speed of 5 ml / h, receiver speed of 1000 rpm, spinning temperature of 25°C, spinning humidity of 35%, and total traction ratio of 30. After spinning, the fibers were collected and placed in a vacuum drying oven at 80°C for 12 h to obtain cobalt-iron-copper modified polymer nanofibers.

[0053] 5mmol of terephthalic acid was added to 80ml of dimethylformamide solution, and the solution was obtained by continuous stirring at room temperature for 20min in a magnetic stirrer at a speed of 500rpm. The fiber membrane cut into a certain size was placed in the solution and allowed to stand for 10 minutes; the fiber and the solution were transferred to a reactor and reacted at 120℃ for 20h. The fiber after the reaction was placed in a methanol solution and washed three times continuously, and placed in a vacuum drying oven at 80℃ for 12h to obtain a polymer nanofiber with a cobalt-iron-copper-based metal organic framework on the surface.

[0054] The fiber was placed in a tubular furnace, heated to 250°C at a heating rate of 1°C / min in an air atmosphere and maintained for 2 hours, and then cooled to room temperature with the furnace. Then, the temperature was raised to 800°C at a heating rate of 1°C / min in an argon atmosphere and maintained for 2 hours, and then cooled to room temperature with the furnace to obtain carbon nanofibers derived from a cobalt-iron-copper-based metal organic framework.

[0055] Example 5

[0056] A multi-level structure transition metal modified carbon nanofiber, the preparation method comprises the following steps:

[0057] 15% by mass of manganese nitrate, iron nitrate, zinc nitrate and copper nitrate (mass ratio 1:1:1:1), 8% by mass of 150,000 molecular weight polyacrylonitrile and 10% by mass of 9,000 molecular weight polyvinyl alcohol were added to dimethylacetamide, and the spinning solution was obtained by continuous stirring at 90°C for 12 hours.

[0058] The spinning solution was added to a 25 ml syringe and spun according to the wet spinning parameters of injection speed of 0.1 ml / h, coagulation bath of a mixed solution of dimethylacetamide and water, receiver speed of 100 rpm, temperature of 20°C, and total traction ratio of 1. After spinning, the fibers were collected and placed in a vacuum drying oven at 60°C for 12 hours to obtain manganese, iron, zinc, and copper modified polymer nanofibers.

[0059] 20 mmol of trimesic acid was added to 80 ml of methanol solution, and the solution was obtained by continuous stirring at room temperature for 20 minutes in a magnetic stirrer at a speed of 500 rpm. The fiber membrane cut into a certain size was placed in the solution and allowed to stand for 10 minutes; the fiber and the solution were transferred to a reactor and reacted at 140°C for 10 hours. The fiber after the reaction was placed in a methanol solution and washed three times continuously, and placed in a vacuum drying oven at 60°C for 12 hours to obtain a polymer nanofiber with a manganese-iron-zinc-copper-based metal organic framework on the surface.

[0060] The fiber was placed in a tubular furnace, heated to 270°C in an air atmosphere at a heating rate of 1°C / min and maintained for 2 hours, and then cooled to room temperature in the furnace. Then, the temperature was raised to 800°C in a nitrogen atmosphere at a heating rate of 1°C / min and maintained for 2 hours, and then cooled to room temperature in the furnace to obtain carbon nanofibers derived from a manganese-iron-zinc-copper-based metal organic framework.

[0061] Example 6

[0062] A multi-level structure transition metal modified carbon nanofiber, the preparation method comprises the following steps:

[0063] 15% by mass of cobalt chloride, ferric chloride and zinc chloride (mass ratio 1:1:1), 5% by mass of 1,300,000 molecular weight polyvinyl pyrrolidone and 10% by mass of 9,000 molecular weight polyvinyl alcohol were added to dimethylacetamide, and the mixture was stirred continuously at 90°C for 5 hours to obtain a spinning solution.

[0064] The spinning solution was added to a 25 ml syringe and spun according to the parameters of injection speed of 0.5 ml / h, distance between syringe needle and receiver of 15 cm, receiver speed of 500 rpm, spinning temperature of 25°C, spinning humidity of 25%, and electrospinning voltage of 17 kV. After spinning, the fibers were collected and placed in a vacuum drying oven at 70°C for 12 hours to obtain cobalt-iron-zinc-modified polymer nanofibers.

[0065] 5g of dimethylimidazole was added to 80ml of methanol solution, and stirred continuously at room temperature for 20min in a magnetic stirrer at 500rpm to obtain a clear solution. The fiber membrane cut into a certain size was placed in the solution, and gently shaken for 30s every 2min and the process lasted for 30min, and finally stood at room temperature for 1h. The reacted fiber was placed in a methanol solution and washed three times continuously, and placed in a vacuum drying oven at 70℃ for 12h to obtain a polymer nanofiber with a cobalt-iron-zinc-based metal organic framework on the surface.

[0066] The fiber was placed in a tubular furnace, heated to 220°C at a heating rate of 1°C / min in an air atmosphere and maintained for 2 hours, and then cooled to room temperature in the furnace. Then, the temperature was raised to 600°C at a heating rate of 1°C / min in a nitrogen atmosphere and maintained for 2 hours, and then cooled to room temperature in the furnace to obtain carbon nanofibers modified with a cobalt-iron-zinc-based metal organic framework.

[0067] In summary, the embodiments of the present invention provide a method for preparing a multi-level structure transition metal modified carbon nanofiber by spinning and hydrothermal method. The preparation method is simple and universal, the fiber function is designable, and it can be applied to the fields of energy, environment, sensing and electromagnetic shielding.

[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing multi-level transition metal modified carbon nanofibers, It is characterized in that The following steps are involved: (1) mixing and dissolving a high carbon yield polymer, a readily soluble polymer, a metal salt and a solvent to obtain a spinning solution; (2) spinning the spinning solution using a spinning process to obtain a transition metal-modified polymer nanofiber precursor; (3) soaking the transition metal modified polymer nanofiber precursor in a solution containing an organic ligand to obtain a multi-level structure transition metal modified polymer nanofiber; (4) calcining and carbonizing the multi-level structure transition metal modified polymer nanofibers to obtain multi-level structure transition metal modified carbon nanofibers.

2. The method for preparing the multi-level transition metal modified carbon nanofiber according to claim 1, It is characterized in that The concentration of the high carbon yield polymer in the spinning solution is 5-10wt%, the concentration of the easily soluble polymer is 5-10wt%, and the concentration of the metal salt is 5-15wt%.

3. The method for preparing the multi-level transition metal modified carbon nanofiber according to claim 2, It is characterized in that The high carbon yield polymer is one or more of polyacrylonitrile with an average molecular weight of 100,000-200,000, polyvinyl pyrrolidone with a molecular weight of 1,000,000-1,300,000, or polyvinyl alcohol with a molecular weight of 85,000-124,000; the easily soluble polymer is polyvinyl pyrrolidone with a molecular weight less than 58,000 or / and polyvinyl alcohol with a molecular weight less than 30,000.

4. The method for preparing the multi-level transition metal modified carbon nanofiber according to claim 3, It is characterized in that The metal salt is any one or more of sulfate, acetate, nitrate, acetylacetonate and chloride; the solvent is any one or more of dimethylacetamide, dimethylformamide and dimethyl sulfoxide.

5. The method for preparing the multi-level transition metal modified carbon nanofiber according to claim 1, It is characterized in that The spinning process is wet spinning, dry spinning or electrostatic spinning.

6. The method for preparing the multi-level transition metal modified carbon nanofiber according to claim 5, It is characterized in that The solution injection speed of the wet spinning or dry spinning is 0.1-5 ml / h, and the total traction ratio is 1-30; the solution injection speed of the electrospinning is 0.1-3 ml / h, the receiver distance is 5-30 cm, the receiver speed is 0-3000 r / min, and the voltage is 5-30 kV.

7. The method for preparing the multi-level transition metal modified carbon nanofiber according to claim 1, It is characterized in that The organic ligand is one or more of dimethylimidazole, terephthalic acid, trimesic acid, etc.; the solvent of the solution containing the organic ligand is one or more of methanol, ethanol and water, and the concentration of the organic ligand is 0.1-0.8M.

8. The method for preparing the multi-level transition metal modified carbon nanofiber according to claim 7, It is characterized in that The soaking method in step (3) is one or more of standing, stirring and ultrasound, and the time is 4-20 hours.

9. The method for preparing the multi-level transition metal modified carbon nanofiber according to claim 1, It is characterized in that The calcination and carbonization steps are: first pre-oxidation at 180-280° C. for 1-3 hours, and then carbonization at 600-1800° C. for 1-3 hours.

10. The multi-level structure transition metal modified carbon nanofiber prepared by the method according to any one of claims 1 to 9.