Moisture-absorbing and sweat-releasing police composite fabric and preparation method thereof
Through alkali solution pretreatment and finishing solution treatment of modified shell powder and glycerin, as well as coating solution treatment of modified scale graphite powder and aqueous epoxy resin, the moisture absorption and sweating and anti-static properties of polyester fiber fabrics are improved, and the solution is solved Polyester fibers have insufficient hygroscopicity and low antistatic properties, and have achieved efficient moisture absorption and sweating and antistatic effects.
Patent Information
- Application Number
- CN202411506218.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyester fibers have poor performance in areas with high requirements for moisture absorption and breathability, resulting in limited application and existing modification methods fail to effectively improve their antistatic properties.
The fabric base cloth was pretreated with alkali solution, and then modified shell powder and glycerin were added to the finishing solution to improve hydrophilic properties through polypyrrole modification treatment; modified scale graphite powder and aqueous epoxy resin were added to the coating solution. The conductive pathway and cross-linking are formed through thermal curing to improve the antistatic and binding strength.
It significantly improves the moisture-wicking and anti-static properties of composite fabrics, maintains good moisture-absorbing and comfort, and still has good performance after multiple washes, enhancing the durability of the fabric.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile materials, and in particular to a moisture-absorbing and perspiration-releasing composite fabric for police use and a preparation method thereof. Background Art
[0002] As people's pursuit of quality of life continues to improve, the requirements for clothing fabrics are no longer limited to the traditional functions of shielding, warmth and protection. Modern consumers pay more and more attention to the versatility and comfort of clothing. For example, they hope that clothing can effectively regulate body temperature and have good moisture absorption and perspiration performance. In daily life, the human body will continue to generate heat, especially when exercising or exposed to high temperature environments, the sweating phenomenon is more obvious. If the moisture after sweating cannot be cleaned or evaporated in time, it is easy to cause bacteria to grow and cause hidden dangers to the skin. Therefore, clothing fabrics need to have good moisture absorption and perspiration functions so that sweat can be quickly absorbed and transferred to the outer surface of the fabric, thereby ensuring the dryness and comfort of the skin surface.
[0003] As one of the three main synthetic fibers, polyester fiber (polyester) has been widely used in clothing fabrics and other non-clothing fields due to its excellent physical and chemical properties. Polyester fiber has the characteristics of high modulus, high strength, good wrinkle resistance, shape retention and heat resistance, so it is very popular in the market. Since its advent, its good drape, high strength, crisp fabric and easy drying have made it the main textile raw material for many downstream users. However, the molecular chain structure of polyester fiber is relatively regular and lacks polar functional groups, which makes its fiber surface too smooth, resulting in poor performance in terms of hygroscopicity. Under standard conditions, the moisture regain of polyester fiber is only 0.4%, which is much lower than the 7.5% of natural cotton fiber. This characteristic makes the application of polyester fiber subject to certain restrictions when it faces fields with high requirements for moisture absorption and breathability.
[0004] In response to the problem of insufficient hygroscopicity of polyester fibers, researchers have carried out a variety of modifications and technological innovations in order to improve their functionality. These methods include introducing hydrophilic additives during the production of polyester fibers, using copolymerization technology or post-treatment processes to increase the polarity and hygroscopicity of the fibers. In addition, in recent years, the application of nanotechnology has also gradually attracted attention. By adding nano-scale materials to polyester fibers, the microstructure of the fabric can be effectively improved, thereby improving the moisture absorption and perspiration performance. These improvements enable polyester fibers to better meet the needs of consumers in areas such as sportswear, outdoor equipment and underwear that require high moisture absorption and perspiration.
[0005] Chinese patent document CN202410452834.X discloses a moisture-absorbing and quick-drying polyester fiber and fabric, which are prepared by polycondensation and spinning of a dibasic acid and a modified diol monomer, wherein the modified diol monomer uses p-alkylphenol as a raw material to introduce an alkyl segment, and introduces a polyether segment through 1-bromo-2-(2-methoxyethoxy)ethane, and then successively introduces a polyhydroxyl group through a bromination reaction and a substitution reaction with phenylboronic acid and a bromide. Through copolymerization modification, a hydrophilic polyether segment and a hydrophobic alkyl segment are simultaneously introduced into the side chain of the polyester resin, on the one hand, the modification compatibility and durability of the polyester resin are improved, and the mechanical properties of the resin body are ensured, and on the other hand, the fiber is given good hygroscopicity and quick-drying properties by adjusting its hydrophilic and hydrophobic properties. However, the antistatic properties of the prepared fabric need to be improved. Summary of the invention
[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a moisture absorbing and perspiration wicking composite fabric for police use and a preparation method thereof.
[0007] In order to achieve the above object, the present invention adopts the following technical scheme: A method for preparing a moisture-absorbing and perspiration-wicking police composite fabric comprises the following steps: S1, immersing the fabric base fabric in an alkaline solution, and then washing and drying the immersed fabric to obtain a pretreated fabric base fabric; S2, immersing the pretreated fabric base in a finishing solution, the finishing solution comprising: deionized water, polyethylene glycol, modified shell powder, glycerol, polyoxyethylene sorbitan monooleate, and sodium lauryl sulfate, and then drying the impregnated fabric to obtain a hygroscopic fabric; S3. Immerse the hygroscopic fabric in a coating liquid, the components of which are: water-based epoxy resin, modified flake graphite powder, sodium carboxymethyl cellulose, and deionized water, and then thermally cure the impregnated fabric to obtain a police composite fabric.
[0008] Specifically, in step S2, the mass ratio of deionized water, polyethylene glycol, modified shell powder, glycerol, polyoxyethylene sorbitan monooleate and sodium lauryl sulfate is 60-80:20-30:8-12:10-15:2-4:2-4.
[0009] Specifically, in step S2, the preparation method of the modified shell powder is as follows: (1) dispersing shell powder in deionized water, adding phosphoric acid and pyrrole, stirring evenly, then adding an oxidant, stirring and reacting to obtain a polypyrrole / shell powder dispersion; (2) Adding the aqueous polyurethane emulsion to the polypyrrole / shell powder dispersion of step (1), and then adding the KH560 hydrolyzate, stirring to react, and after the reaction is completed, freeze-drying and grinding to obtain the modified shell powder.
[0010] Specifically, in step (1), the mass ratio of shell powder, deionized water, phosphoric acid, pyrrole and oxidant is 5-10:100:1-2:4-8:3-6, wherein the oxidant is selected from ammonium persulfate or sodium persulfate.
[0011] Specifically, in step (2), the mass ratio of the aqueous polyurethane emulsion, the polypyrrole / shell powder dispersion and the KH560 hydrolyzate is 1-1.5:1:0.3-0.5, wherein the mass fraction of the KH560 hydrolyzate is 10-15%.
[0012] Specifically, in step S3, the mass ratio of waterborne epoxy resin, modified flake graphite powder, sodium carboxymethyl cellulose and deionized water is 40-60:3-5:1-2:10-20.
[0013] Specifically, the preparation method of the modified flake graphite powder is as follows: (01) immersing the flake graphite powder in an alkaline solution, performing ultrasonic dispersion treatment, and then washing with deionized water and drying to obtain pretreated flake graphite powder; (02) Dispersing the pretreated flake graphite powder in deionized water, then adding aminoacetonitrile hydrochloride and epichlorohydrin, heating and stirring at 60-80°C for 2-4 hours, filtering, washing and drying the reaction product to obtain modified flake graphite powder.
[0014] Specifically, in step (02), the mass ratio of pretreated flake graphite powder, aminoacetonitrile hydrochloride and epichlorohydrin is 8-12:3-5:2-4.
[0015] Specifically, in step S3, the thermal curing temperature is 70-80° C., and the thermal curing time is 2-3 hours.
[0016] The present invention also provides a police composite fabric prepared by the above preparation method.
[0017] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention first uses an alkaline solution to pretreat the fabric base fabric, which can effectively remove impurities and grease on the surface of the fabric base fabric, and at the same time increase the surface roughness and hydroxyl content of the fabric base fabric, which is beneficial to the adsorption of subsequent finishing liquid.
[0018] (2) The present invention utilizes polypyrrole to modify the shell powder, thereby improving the antistatic properties of the shell powder, and further improving the antistatic properties of the composite fabric; polypyrrole is coated on the surface of the shell powder, which is not conducive to the moisture absorption of the shell powder. The present invention utilizes the epoxy functional group on KH560 to undergo a ring-opening reaction with the amino group on the waterborne polyurethane, and grafts the waterborne polyurethane on the surface of the polypyrrole / shell powder, significantly improving its hydrophilic properties, thereby allowing the fabric to maintain good moisture absorption and perspiration function.
[0019] (3) The finishing liquid provided by the present invention contains polyethylene glycol, modified shell powder and glycerol. The hydrophilicity of polyethylene glycol, modified shell powder and glycerol enables the fabric to quickly absorb sweat and discharge it, keeping the wearer dry and comfortable. In addition, the addition of glycerol can also increase the softness of the fabric, further improving the wearing comfort experience.
[0020] (4) The present invention grafts aminoacetonitrile hydrochloride onto the surface of flake graphite powder through the cross-linking effect of epichlorohydrin, thereby improving the hygroscopic properties of the flake graphite powder. At the same time, the flake graphite powder and polypyrrole form a conductive path, further improving the antistatic effect of the fabric. During the thermal curing process, the epoxy groups in the water-based epoxy resin can cross-link with the hydroxyl groups in polyethylene glycol and glycerol, and the amino groups in the modified shell powder and modified flake graphite powder, thereby improving their bonding strength and effectively preventing the hygroscopic components from falling off the surface of the fabric. After multiple washings, the fabric still has good hygroscopic and antistatic properties. DETAILED DESCRIPTION
[0021] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.
[0022] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.
[0023] A method for preparing a moisture-absorbing and perspiration-wicking police composite fabric comprises the following steps: S1. Preparation of pre-treated fabric base fabric The fabric base cloth is immersed in an alkaline solution, and then the immersed fabric is washed and dried to obtain a pretreated fabric base cloth.
[0024] In the technical solution of the present invention, the fabric base fabric is selected from polyester or nylon.
[0025] The alkaline solution is selected from sodium hydroxide solution or potassium hydroxide solution, and the concentration of the alkaline solution is 0.5-2 mol / L, for example, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] In the technical solution of the present invention, the immersion treatment temperature is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C, and 80°C can be selected; the immersion treatment time is 2-5h, for example, 2h, 3h, 4h, and 5h can be selected; but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] In this step, by pretreating the fabric base fabric with an alkaline solution, impurities and grease on the surface of the fabric base fabric can be effectively removed, and the surface roughness and hydroxyl content of the fabric base fabric can be increased, which is beneficial to the adsorption of the subsequent finishing liquid.
[0028] S2. Preparation of moisture-absorbing fabric The pretreated fabric base cloth is immersed in a finishing liquid, the ingredients of which are: deionized water, polyethylene glycol, modified shell powder, glycerol, polyoxyethylene sorbitan monooleate, and sodium dodecyl sulfate, and then the immersed fabric is dried to obtain a hygroscopic fabric.
[0029] In this step, the bath ratio of the pretreated fabric base cloth and the finishing liquid is 1:10-15, for example, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15 can be selected; but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] In this step, the padding liquid rate of the pre-treated fabric base fabric is 70-80%.
[0031] In the technical solution of the present invention, the mass ratio of deionized water, polyethylene glycol, modified shell powder, glycerol, polyoxyethylene sorbitan monooleate and sodium lauryl sulfate in the finishing liquid is 60-80:20-30:8-12:10-15:2-4:2-4.
[0032] Wherein, the preparation method of modified shell powder is as follows: (1) dispersing shell powder in deionized water, adding phosphoric acid and pyrrole, stirring evenly, then adding an oxidant, stirring and reacting to obtain a polypyrrole / shell powder dispersion; (2) Adding the aqueous polyurethane emulsion to the polypyrrole / shell powder dispersion of step (1), and then adding the KH560 hydrolyzate, stirring to react, and after the reaction is completed, freeze-drying and grinding to obtain the modified shell powder.
[0033] In the technical solution of the present invention, in step (1), the mass ratio of shell powder, deionized water, phosphoric acid, pyrrole and oxidant is 5-10:100:1-2:4-8:3-6.
[0034] The oxidizing agent is selected from ammonium persulfate or sodium persulfate.
[0035] In step (1), the stirring reaction time is 12-18 hours, for example, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours can be selected, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0036] In step (2), the mass ratio of the aqueous polyurethane emulsion, the polypyrrole / shell powder dispersion and the KH560 hydrolyzate is 1-1.5:1:0.3-0.5.
[0037] The preparation method of KH560 hydrolyzate is as follows: adding silane coupling agent KH560 to 80wt% ethanol aqueous solution, stirring at room temperature for 2h, and obtaining KH560 hydrolyzate.
[0038] In the technical solution of the present invention, the mass fraction of KH560 hydrolyzate is 10-15%.
[0039] In step (2), the stirring reaction time is 2-4 hours.
[0040] In the technical scheme of the present invention, although shell powder has good hygroscopic properties, its antistatic properties are poor. The present invention utilizes polypyrrole to modify the shell powder, thereby improving the antistatic properties of the shell powder, and further improving the antistatic properties of the composite fabric; polypyrrole is coated on the surface of the shell powder, which is not conducive to the moisture absorption of the shell powder. The present invention utilizes the epoxy functional group on KH560 to undergo a ring-opening reaction with the amino group on the water-based polyurethane, and grafts the water-based polyurethane on the surface of the polypyrrole / shell powder, thereby significantly improving its hydrophilic properties, thereby allowing the fabric to maintain good moisture absorption and perspiration functions.
[0041] In the technical solution of the present invention, the finishing liquid contains polyethylene glycol, modified shell powder and glycerin. The hydrophilicity of polyethylene glycol, modified shell powder and glycerin enables the fabric to quickly absorb sweat and discharge it, keeping the wearer dry and comfortable; in addition, the addition of glycerin can also increase the softness of the fabric, further enhancing the wearing comfort experience.
[0042] S3. Preparation of police composite fabrics The hygroscopic fabric is immersed in a coating liquid whose ingredients are: water-based epoxy resin, modified flake graphite powder, sodium carboxymethyl cellulose, and deionized water. The immersed fabric is then thermally cured to obtain a police composite fabric.
[0043] In this step, the bath ratio of the hygroscopic fabric and the coating liquid is 1:10-15, for example, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15 can be selected; but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] In this step, the padding liquid rate of the hygroscopic fabric is 70-80%.
[0045] In the technical solution of the present invention, the mass ratio of water-based epoxy resin, modified flake graphite powder, sodium carboxymethyl cellulose and deionized water in the coating liquid is 40-60:3-5:1-2:10-20.
[0046] Wherein, the preparation method of modified flake graphite powder is as follows: (01) immersing the flake graphite powder in an alkaline solution, performing ultrasonic dispersion treatment, and then washing with deionized water and drying to obtain pretreated flake graphite powder; (02) Dispersing the pretreated flake graphite powder in deionized water, then adding aminoacetonitrile hydrochloride and epichlorohydrin, heating and stirring at 60-80°C for 2-4 hours, filtering, washing and drying the reaction product to obtain modified flake graphite powder.
[0047] In the technical solution of the present invention, in step (01), the alkaline solution is selected from sodium hydroxide solution or potassium hydroxide solution, and the concentration of the alkaline solution is 0.5-2 mol / L, for example, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L can be selected, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0048] In step (01), the power of ultrasonic dispersion is 400-600 W, for example, 400 W, 450 W, 500 W, 550 W, and 600 W can be selected; the time of ultrasonic dispersion is 1-3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h, and 3 h can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0049] In step (02), the mass ratio of pretreated flake graphite powder, aminoacetonitrile hydrochloride and epichlorohydrin is 8-12:3-5:2-4.
[0050] In the technical solution of the present invention, the thermal curing temperature is 70-80°C, for example, 70°C, 72°C, 74°C, 75°C, 76°C, 78°C, and 80°C can be selected; the thermal curing time is 2-3h, for example, 2h, 2.5h, and 3h can be selected; but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0051] In the technical scheme of the present invention, considering that components such as polyethylene glycol, modified shell powder and glycerol are easy to fall off from the surface of the fabric base cloth, resulting in a decrease in the hygroscopic performance of the fabric, the present invention loads a coating layer on the surface of the hygroscopic fabric to prevent the hygroscopic components from falling off the surface of the fabric; in the coating layer, aminoacetonitrile hydrochloride is first grafted on the surface of the flake graphite powder through the cross-linking effect of epichlorohydrin, thereby improving the hygroscopic performance of the flake graphite powder. At the same time, the flake graphite powder and polypyrrole form a conductive path, further improving the antistatic effect of the composite fabric; in the process of thermal curing, the epoxy groups in the water-based epoxy resin can cross-link with the hydroxyl groups in polyethylene glycol and glycerol, and the amino groups in the modified shell powder and modified flake graphite powder, thereby improving their bonding strength and effectively preventing the hygroscopic components from falling off the surface of the fabric. After multiple washings, the fabric still has good hygroscopic performance.
[0052] The present invention is further illustrated below by means of specific embodiments, wherein the model of polyethylene glycol is polyethylene glycol 400, the mesh number of shell powder is 2000 mesh, the model of waterborne polyurethane emulsion is PU667, purchased from Nanjing Chuhai New Material Technology Co., Ltd., the brand of waterborne epoxy resin is CYDW-100, and the mesh number of flake graphite powder is 1250 mesh.
[0053] Example 1
[0054] A method for preparing a moisture-absorbing and perspiration-wicking police composite fabric comprises the following steps: S1. Immerse the polyester fabric base cloth in a 1 mol / L sodium hydroxide solution with a bath ratio of 1:10. The immersion treatment temperature is 60° C. and the immersion treatment time is 5 h. Then, the immersed fabric is washed and dried to obtain a pretreated fabric base cloth.
[0055] S2, immersing the pretreated fabric base fabric in a finishing solution with a bath ratio of 1:10, wherein the finishing solution comprises: 60 parts of deionized water, 20 parts of polyethylene glycol, 8 parts of modified shell powder, 10 parts of glycerol, 2 parts of polyoxyethylene sorbitan monooleate and 2 parts of sodium lauryl sulfate, and then taking out the padding treated fabric, with a padding liquid rate of 70%, and then drying at 50°C to obtain a hygroscopic fabric; Wherein, the preparation method of modified shell powder is as follows: (1) Disperse 5 g of shell powder in 100 g of deionized water, add 1 g of phosphoric acid and 4 g of pyrrole, stir evenly, then add 3 g of oxidant ammonium persulfate, stir and react for 12 h to obtain a polypyrrole / shell powder dispersion; (2) Add 10 g of aqueous polyurethane emulsion to 10 g of the polypyrrole / shell powder dispersion of step (1), and then add 3 g of KH560 hydrolyzate, where the mass fraction of KH560 hydrolyzate is 10%, and stir to react for 3 h. After the reaction is completed, freeze-dry and grind to obtain modified shell powder.
[0056] S3, immersing the hygroscopic fabric in a coating liquid with a bath ratio of 1:10, the composition of the coating liquid is: 40 parts of water-based epoxy resin, 3 parts of modified flake graphite powder, 1 part of sodium carboxymethyl cellulose and 10 parts of deionized water, then taking out the fabric after padding treatment, the padding liquid rate is 70%, and then thermally curing the impregnated fabric at 70°C for 3h to obtain a police composite fabric; Wherein, the preparation method of modified flake graphite powder is as follows: (01) 10 g of flake graphite powder was immersed in 100 mL of 1 mol / L sodium hydroxide solution, and subjected to ultrasonic dispersion treatment at an ultrasonic power of 400 W for 3 h, followed by washing with deionized water and drying to obtain pretreated flake graphite powder; (02) Disperse 8 g of pretreated flake graphite powder in 100 g of deionized water, then add 3 g of aminoacetonitrile hydrochloride and 2 g of epichlorohydrin, heat and stir at 60 °C for 4 h, filter, wash and dry the reaction product to obtain modified flake graphite powder.
[0057] Example 2
[0058] A method for preparing a moisture-absorbing and perspiration-wicking police composite fabric comprises the following steps: S1. Immerse the polyester fabric base cloth in a 1 mol / L sodium hydroxide solution with a bath ratio of 1:10. The immersion treatment temperature is 80° C. and the immersion treatment time is 2 h. Then, the immersed fabric is washed and dried to obtain a pretreated fabric base cloth.
[0059] S2, immersing the pretreated fabric base fabric in a finishing solution with a bath ratio of 1:15, wherein the finishing solution comprises: 80 parts of deionized water, 30 parts of polyethylene glycol, 12 parts of modified shell powder, 15 parts of glycerol, 4 parts of polyoxyethylene sorbitan monooleate and 4 parts of sodium lauryl sulfate, and then taking out the padding treated fabric, with a padding liquid rate of 70%, and then drying at 50°C to obtain a hygroscopic fabric; Wherein, the preparation method of modified shell powder is as follows: (1) Disperse 10 g of shell powder in 100 g of deionized water, add 2 g of phosphoric acid and 8 g of pyrrole, stir evenly, then add 6 g of oxidant ammonium persulfate, stir and react for 18 h to obtain a polypyrrole / shell powder dispersion; (2) Add 15 g of aqueous polyurethane emulsion to 10 g of the polypyrrole / shell powder dispersion of step (1), and then add 5 g of KH560 hydrolyzate, where the mass fraction of KH560 hydrolyzate is 15%, and stir to react for 4 h. After the reaction is completed, freeze-dry and grind to obtain modified shell powder.
[0060] S3, immersing the hygroscopic fabric in a coating liquid with a bath ratio of 1:10, the composition of the coating liquid is: 60 parts of waterborne epoxy resin, 5 parts of modified flake graphite powder, 2 parts of sodium carboxymethyl cellulose and 20 parts of deionized water, then taking out the fabric after padding treatment, the padding liquid rate is 70%, and then heat curing the impregnated fabric at 80°C for 2h to obtain a police composite fabric; Wherein, the preparation method of modified flake graphite powder is as follows: (01) 10 g of flake graphite powder was immersed in 100 mL of 1 mol / L sodium hydroxide solution, and subjected to ultrasonic dispersion treatment at an ultrasonic power of 600 W and an ultrasonic time of 1 h, followed by washing with deionized water and drying to obtain pretreated flake graphite powder; (02) Disperse 12 g of pretreated flake graphite powder in 100 g of deionized water, then add 5 g of aminoacetonitrile hydrochloride and 4 g of epichlorohydrin, heat and stir at 80 °C for 2 h, filter, wash and dry the reaction product to obtain modified flake graphite powder.
[0061] Example 3
[0062] A method for preparing a moisture-absorbing and perspiration-wicking police composite fabric comprises the following steps: S1. Immerse the polyester fabric base cloth in 1 mol / L sodium hydroxide solution with a bath ratio of 1:10. The immersion treatment temperature is 70° C. and the immersion treatment time is 4 h. Then, wash and dry the immersed fabric to obtain a pretreated fabric base cloth.
[0063] S2, immersing the pretreated fabric base fabric in a finishing solution with a bath ratio of 1:10, wherein the finishing solution comprises: 70 parts of deionized water, 24 parts of polyethylene glycol, 10 parts of modified shell powder, 12 parts of glycerol, 2 parts of polyoxyethylene sorbitan monooleate and 3 parts of sodium lauryl sulfate, and then taking out the padding treated fabric, with a padding liquid rate of 70%, and then drying at 50°C to obtain a hygroscopic fabric; Wherein, the preparation method of modified shell powder is as follows: (1) 8 g of shell powder was dispersed in 100 g of deionized water, 2 g of phosphoric acid and 6 g of pyrrole were added, and the mixture was stirred evenly. Then, 5 g of oxidant ammonium persulfate was added, and the mixture was stirred for 15 h to obtain a polypyrrole / shell powder dispersion; (2) Add 12 g of aqueous polyurethane emulsion to 10 g of the polypyrrole / shell powder dispersion of step (1), and then add 4 g of KH560 hydrolyzate, where the mass fraction of KH560 hydrolyzate is 15%, and stir to react for 3 h. After the reaction is completed, freeze-dry and grind to obtain modified shell powder.
[0064] S3, immersing the hygroscopic fabric in a coating liquid with a bath ratio of 1:15, the composition of the coating liquid is: 50 parts of water-based epoxy resin, 4 parts of modified flake graphite powder, 2 parts of sodium carboxymethyl cellulose and 15 parts of deionized water, then taking out the fabric after padding treatment, the padding liquid rate is 70%, and then heat curing the impregnated fabric at 80°C for 2h to obtain a police composite fabric; Wherein, the preparation method of modified flake graphite powder is as follows: (01) 10 g of flake graphite powder was immersed in 100 mL of 1 mol / L sodium hydroxide solution, and subjected to ultrasonic dispersion treatment at an ultrasonic power of 500 W for 2 h, followed by washing with deionized water and drying to obtain pretreated flake graphite powder; (02) Disperse 10 g of pretreated flake graphite powder in 100 g of deionized water, then add 4 g of aminoacetonitrile hydrochloride and 4 g of epichlorohydrin, heat and stir at 80 °C for 2 h, filter, wash and dry the reaction product to obtain modified flake graphite powder.
[0065] Comparative Example 1
[0066] A method for preparing a moisture-absorbing and perspiration-wicking police composite fabric comprises the following steps: S1. Immerse the polyester fabric base cloth in a 1 mol / L sodium hydroxide solution with a bath ratio of 1:10. The immersion treatment temperature is 60° C. and the immersion treatment time is 5 h. Then, the immersed fabric is washed and dried to obtain a pretreated fabric base cloth.
[0067] S2. Immerse the pretreated fabric base in the finishing liquid with a bath ratio of 1:10, wherein the finishing liquid comprises 60 parts of deionized water, 20 parts of polyethylene glycol, 8 parts of shell powder, 10 parts of glycerol, 2 parts of polyoxyethylene sorbitan monooleate and 2 parts of sodium lauryl sulfate, and then take out the fabric after padding treatment, with a padding liquid rate of 70%, and then dry at 50°C to obtain a hygroscopic fabric.
[0068] S3, immersing the hygroscopic fabric in a coating liquid with a bath ratio of 1:10, the composition of the coating liquid is: 40 parts of water-based epoxy resin, 3 parts of modified flake graphite powder, 1 part of sodium carboxymethyl cellulose and 10 parts of deionized water, then taking out the fabric after padding treatment, the padding liquid rate is 70%, and then thermally curing the impregnated fabric at 70°C for 3h to obtain a police composite fabric; Wherein, the preparation method of modified flake graphite powder is as follows: (01) 10 g of flake graphite powder was immersed in 100 mL of 1 mol / L sodium hydroxide solution, and subjected to ultrasonic dispersion treatment at an ultrasonic power of 400 W for 3 h, followed by washing with deionized water and drying to obtain pretreated flake graphite powder; (02) Disperse 8 g of pretreated flake graphite powder in 100 g of deionized water, then add 3 g of aminoacetonitrile hydrochloride and 2 g of epichlorohydrin, heat and stir at 60 °C for 4 h, filter, wash and dry the reaction product to obtain modified flake graphite powder.
[0069] Compared with Example 1, Comparative Example 1 did not perform modification treatment on the shell powder.
[0070] Comparative Example 2
[0071] A method for preparing a moisture-absorbing and perspiration-wicking police composite fabric comprises the following steps: S1. Immerse the polyester fabric base cloth in a 1 mol / L sodium hydroxide solution with a bath ratio of 1:10. The immersion treatment temperature is 60° C. and the immersion treatment time is 5 h. Then, the immersed fabric is washed and dried to obtain a pretreated fabric base cloth.
[0072] S2, immersing the pretreated fabric base fabric in a finishing solution with a bath ratio of 1:10, wherein the finishing solution comprises: 60 parts of deionized water, 20 parts of polyethylene glycol, 8 parts of modified shell powder, 10 parts of glycerol, 2 parts of polyoxyethylene sorbitan monooleate and 2 parts of sodium lauryl sulfate, and then taking out the padding treated fabric, with a padding liquid rate of 70%, and then drying at 50°C to obtain a hygroscopic fabric; Wherein, the preparation method of modified shell powder is as follows: (1) Disperse 5 g of shell powder in 100 g of deionized water, add 1 g of phosphoric acid and 4 g of pyrrole, stir evenly, then add 3 g of oxidant ammonium persulfate, stir and react for 12 h to obtain a polypyrrole / shell powder dispersion; (2) Add 10 g of aqueous polyurethane emulsion to 10 g of the polypyrrole / shell powder dispersion of step (1), and then add 3 g of KH560 hydrolyzate, where the mass fraction of KH560 hydrolyzate is 10%, and stir to react for 3 h. After the reaction is completed, freeze-dry and grind to obtain modified shell powder.
[0073] S3. Immerse the hygroscopic fabric in the coating liquid with a bath ratio of 1:10. The components of the coating liquid are: 40 parts of water-based epoxy resin, 3 parts of flake graphite powder, 1 part of sodium carboxymethyl cellulose and 10 parts of deionized water. Then take out the fabric after the padding treatment. The padding liquid rate is 70%. Then, heat cure the impregnated fabric at 70°C for 3 hours to obtain a police composite fabric.
[0074] Compared with Example 1, in Comparative Example 2, no modification treatment was performed on the flake graphite powder.
[0075] Comparative Example 3
[0076] A method for preparing a moisture-absorbing and perspiration-wicking police composite fabric comprises the following steps: S1. Immerse the polyester fabric base cloth in a 1 mol / L sodium hydroxide solution with a bath ratio of 1:10. The immersion treatment temperature is 60° C. and the immersion treatment time is 5 h. Then, the immersed fabric is washed and dried to obtain a pretreated fabric base cloth.
[0077] S2, immersing the pretreated fabric base fabric in a finishing solution with a bath ratio of 1:10, wherein the finishing solution comprises: 60 parts of deionized water, 20 parts of polyethylene glycol, 8 parts of modified shell powder, 10 parts of glycerol, 2 parts of polyoxyethylene sorbitan monooleate and 2 parts of sodium lauryl sulfate, and then taking out the padding treated fabric, with a padding liquid rate of 70%, and then drying at 50°C to obtain a police composite fabric; Wherein, the preparation method of modified shell powder is as follows: (1) Disperse 5 g of shell powder in 100 g of deionized water, add 1 g of phosphoric acid and 4 g of pyrrole, stir evenly, then add 3 g of oxidant ammonium persulfate, stir and react for 12 h to obtain a polypyrrole / shell powder dispersion; (2) Add 10 g of aqueous polyurethane emulsion to 10 g of the polypyrrole / shell powder dispersion of step (1), and then add 3 g of KH560 hydrolyzate, where the mass fraction of KH560 hydrolyzate is 10%, and stir to react for 3 h. After the reaction is completed, freeze-dry and grind to obtain modified shell powder.
[0078] Compared with Example 1, Comparative Example 3 omitted the experimental step of immersing the hygroscopic fabric in the coating liquid.
[0079] The composite fabrics prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests, as follows: Moisture permeability: Tested in accordance with GB / T 12704.2-2009 "Test method for moisture permeability of textile fabrics - Part 2: Evaporation method"; Stiffness: Tested in accordance with GB / T 8318.1-2009, the smaller the stiffness value, the softer the fabric; Surface charge density test: The test is conducted using the charge surface density method in the national standard GB / T 12703.3-2009; The test results are shown in Table 1: Table 1 Performance test table of the composite fabrics prepared in Examples 1-3 and Comparative Examples 1-3
[0080] The composite fabrics prepared in Example 1 and Comparative Example 3 were washed 30 times with standard water, and then the performance test was performed. The standard washing method was as follows: the standard detergent dosage was 2 g / L, the washing condition was 40°C, the washing was performed in a household washing machine, the washing time was 5 minutes, and the composite fabrics were dried in an oven at 60°C, and the total washing time was 30 times. The test results are shown in Table 2: Table 2 Performance test table of the composite fabrics prepared in Example 1 and Comparative Example 3 after 30 standard washes
[0081] It can be seen from the table that the composite fabric prepared by the present invention has good water washing resistance, and after being washed 30 times, it still has good hygroscopicity and antistatic properties.
[0082] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.
Claims
1. A method for preparing a moisture-absorbing and perspiration-wicking police composite fabric, characterized in that: The steps include: S1, immersing the fabric base fabric in an alkaline solution, and then washing and drying the immersed fabric to obtain a pretreated fabric base fabric; S2, immersing the pretreated fabric base in a finishing solution, the finishing solution comprising: deionized water, polyethylene glycol, modified shell powder, glycerol, polyoxyethylene sorbitan monooleate, and sodium lauryl sulfate, and then drying the impregnated fabric to obtain a hygroscopic fabric; S3. Immerse the hygroscopic fabric in a coating liquid, the components of which are: water-based epoxy resin, modified flake graphite powder, sodium carboxymethyl cellulose, and deionized water, and then thermally cure the impregnated fabric to obtain a police composite fabric.
2. The preparation method according to claim 1, characterized in that: In step S2, the mass ratio of deionized water, polyethylene glycol, modified shell powder, glycerol, polyoxyethylene sorbitan monooleate and sodium lauryl sulfate is 60-80:20-30:8-12:10-15:2-4:2-4.
3. The preparation method according to claim 1, characterized in that: In step S2, the preparation method of the modified shell powder is as follows: (1) dispersing shell powder in deionized water, adding phosphoric acid and pyrrole, stirring evenly, then adding an oxidant, stirring and reacting, and obtaining a polypyrrole / shell powder dispersion; (2) Adding the aqueous polyurethane emulsion to the polypyrrole / shell powder dispersion of step (1), and then adding the KH560 hydrolyzate, stirring to react, and after the reaction is completed, freeze-drying and grinding to obtain the modified shell powder.
4. The preparation method according to claim 3, characterized in that: In step (1), the mass ratio of shell powder, deionized water, phosphoric acid, pyrrole and oxidant is 5-10:100:1-2:4-8:3-6, wherein the oxidant is selected from ammonium persulfate or sodium persulfate.
5. The preparation method according to claim 3, characterized in that: In step (2), the mass ratio of the aqueous polyurethane emulsion, the polypyrrole / shell powder dispersion and the KH560 hydrolyzate is 1-1.5:1:0.3-0.5, wherein the mass fraction of the KH560 hydrolyzate is 10-15%.
6. The preparation method according to claim 1, characterized in that: In step S3, the mass ratio of waterborne epoxy resin, modified flake graphite powder, sodium carboxymethyl cellulose and deionized water is 40-60:3-5:1-2:10-20.
7. The preparation method according to claim 6, characterized in that: The preparation method of the modified flake graphite powder is as follows: (01) immersing the flake graphite powder in an alkaline solution, performing ultrasonic dispersion treatment, and then washing with deionized water and drying to obtain pretreated flake graphite powder; (02) Dispersing the pretreated flake graphite powder in deionized water, then adding aminoacetonitrile hydrochloride and epichlorohydrin, heating and stirring at 60-80°C for 2-4 hours, filtering, washing and drying the reaction product to obtain modified flake graphite powder.
8. The preparation method according to claim 6, characterized in that: In step (02), the mass ratio of pretreated flake graphite powder, aminoacetonitrile hydrochloride and epichlorohydrin is 8-12:3-5:2-4.
9. The preparation method according to claim 1, characterized in that: In step S3, the thermal curing temperature is 70-80°C and the thermal curing time is 2-3h.
10. The police composite fabric prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Fabric with moisture absorption and sweat releasing functions and preparation method thereof
CN116752270A