Wear-resistant and noise-reducing artificial leather material and preparation method thereof

By using carrier resin with specific ratios, silicone elastomer microparticles and other raw materials in artificial leather materials, the problems of insufficient wear resistance and high friction noise are solved, and the wear resistance and noise reduction effect are improved. Get a ride experience.

CN119041218APending Publication Date: 2024-11-29KUSN ACHILLES ARTIFICIAL LEATHER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411360322.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

While maintaining wear resistance, existing artificial leather materials are difficult to effectively reduce friction noise, affecting the attention and ride experience of drivers and passengers.

Method used

The raw materials such as carrier resin, silicone elastomer microparticles with grafted polar groups, bridge agents, noise reduction additives, epoxy soybean oil acrylate and glucomannan are processed through specific ratios and processes. Prepare wear-resistant and noise-reducing artificial leather materials, optimize the coating structure, reduce friction noise and improve the material's wear resistance and auditory experience.

Benefits of technology

It realizes artificial leather materials with excellent wear resistance and effectively reduce friction noise, which improves user's auditory experience and ride comfort, has a simple process and high production efficiency, and reduces the phenomenon of agglomeration and stratification in traditional processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005064778290000071
    Figure BDA0005064778290000071
  • Figure BDA0005064778290000081
    Figure BDA0005064778290000081
Patent Text Reader

Abstract

The invention relates to the technical field of artificial leather materials. The invention discloses a wear-resistant and noise-reducing artificial leather material and a preparation method thereof. The artificial leather material comprises an artificial leather base material and a surface treating agent coated on the surface of the artificial leather base material; the surface treating agent comprises carrier resin, organic silicon elastomer micron particles grafted with polar groups, a bridging agent, a noise reduction additive, color paste, epoxidized soybean oil acrylate and glucomannan. The preparation method comprises the following steps that S1, raw materials are sequentially mixed, stirred, dispersed and defoamed, and a surface treating agent is prepared; s2, cleaning an artificial leather base material; s3, the surface of an artificial leather base material is coated with the surface treating agent in a roller coating mode, drying, heat treatment and cooling are conducted, and the wear-resisting and noise-reducing artificial leather material is prepared. The artificial leather material prepared in the invention has excellent wear resistance, and can effectively reduce friction noise.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of artificial leather materials, and in particular to a wear-resistant and noise-reducing artificial leather material and a preparation method thereof. Background Art

[0002] With the continuous progress of the modern automobile industry, especially the rapid development of new energy vehicles, the design concept of car cockpits is also constantly innovating. In the past, car cockpit design mainly focused on functionality and durability, but now, consumers' requirements for the interior environment of the vehicle have shifted from traditional high performance to a comprehensive experience that combines high performance with high perception. This shift is reflected in the comprehensive consideration of multiple dimensions such as material vision (such as color, pattern, gloss), taste (such as odor), hearing (such as noise), and touch (such as stickiness, elasticity, hardness, surface temperature and roughness), reflecting the market's higher expectations for the overall quality of car interiors.

[0003] At present, the development of automotive interior materials is characterized by diversification and personalization. The application of a variety of new materials and new processes enables the interior to better meet the user's needs for beauty, comfort and environmental protection. For example, artificial leather, as an important interior material, has reached a high standard in terms of vision and touch, can simulate the effect close to natural leather, and provides a variety of style options to meet the design needs of different models.

[0004] Nevertheless, while pursuing visual and tactile effects, most of the existing artificial leather materials on the market still have obvious deficiencies in auditory experience. In particular, in terms of reducing the noise generated by material friction, existing technical solutions are difficult to meet market demand. Specifically, when artificial leather is used in car seats, door panels or dashboards, the noise generated by the mutual friction between materials during long-term use not only affects the attention and emotions of drivers and passengers, but also reduces the overall riding experience. This phenomenon shows that the existing technology has failed to effectively solve the problem of friction noise while maintaining the wear resistance of the material.

[0005] Therefore, there is an urgent need to develop an artificial leather material with excellent wear resistance and capable of effectively reducing friction noise, thereby providing users with a quieter and more comfortable riding environment. Summary of the invention

[0006] In order to solve at least one of the above technical problems, an artificial leather material with excellent wear resistance and effective friction noise reduction is developed. The present application provides a wear-resistant and noise-reducing artificial leather material and a preparation method thereof.

[0007] On the one hand, the present application provides a wear-resistant and noise-reducing artificial leather material, comprising an artificial leather base material and a surface treatment agent coated on the surface of the artificial leather base material; the surface treatment agent comprises 90 to 110 parts of a carrier resin, 1 to 15 parts of silicone elastomer micron particles grafted with polar groups, 5 to 10 parts of a bridging agent, 1 to 10 parts of a noise reduction aid, 5 to 10 parts of a color paste, 5 to 10 parts of epoxy soybean oil acrylate, and 0.5 to 1 part of glucomannan.

[0008] By adopting the above technical scheme, the present application adopts specific raw materials and proportions to produce artificial leather materials with excellent wear resistance and can effectively reduce friction noise. The present application adds a carrier resin with excellent wear resistance and silicone elastomer micron particles with excellent noise reduction performance to optimize the microstructure of the coating, reduce the friction noise between materials, and enhance the user's auditory experience. The addition of a bridging agent in the present application can promote the cross-linking reaction between resin molecules and improve the hardness and wear resistance of the coating; the noise reduction aid can reduce friction noise and provide a lubricating effect; the addition of epoxy soybean oil acrylate in the present application can improve the flexibility and adhesion of the coating, while participating in the cross-linking reaction and optimizing the coating performance. The addition of glucomannan in the present application improves the rheological properties of the coating, increases the stability of the coating, and further improves the wear resistance and noise reduction performance of the material.

[0009] Optionally, the carrier resin is selected from one of polyurethane resin, acrylic resin and polyester resin.

[0010] By adopting the above technical solution, the carrier resin of the present application can provide excellent wear resistance and flexibility, and can also improve adhesion, ensuring that the coating is not easy to fall off even in complex environments.

[0011] Optionally, in the organosilicon elastomer microparticles grafted with polar groups, the polar groups are one of hydroxyl, amino and carboxyl groups.

[0012] By adopting the above technical solution, the present application grafts polar groups on the silicone elastomer micron particles to form a more stable network structure, improve wear resistance, enhance adhesion, and improve dispersion uniformity.

[0013] Optionally, the organosilicon elastomer microparticles grafted with polar groups account for 3-7% of the total amount of the surface treatment agent.

[0014] By adopting the above technical solution, the content of the organosilicon elastomer microparticles grafted with polar groups in the present application further improves the wear resistance and surface friction properties, thereby reducing friction noise.

[0015] Optionally, the bridging agent is selected from at least one of isocyanate, epoxy resin and titanate.

[0016] By adopting the above technical solution, the bridging agent of the present application can improve the wear resistance and adhesion of the material.

[0017] Optionally, the noise reduction agent is selected from at least one of polyethylene wax, dimethyl polysiloxane, and polytetrafluoroethylene.

[0018] By adopting the above technical solution, the noise reduction additive of the present application can reduce the friction between material surfaces, significantly reduce friction noise, and can also improve the surface hardness and wear resistance of the coating and reduce wear.

[0019] Optionally, the average particle size of the noise reduction agent is 0.1 to 10 μm.

[0020] By adopting the above technical solution, the average particle size of the noise reduction agent of the present application ensures the dispersibility and function maximization of the noise reduction agent in the coating, and the fine noise reduction agent can form a finer lubricating layer on the coating surface to reduce friction noise.

[0021] Optionally, the weight ratio of the epoxy soybean oil acrylate to glucomannan is 8 to 12:1.

[0022] By adopting the above technical solution, the epoxy soybean oil acrylate and glucomannan work together to improve the stability of the coating, making the coating more stable during storage and use, and not easy to delaminate or settle. It also improves the lubricity of the coating, reduces friction, and reduces friction noise.

[0023] In a second aspect, the present application provides a method for preparing the above-mentioned wear-resistant and noise-reducing artificial leather material, comprising the following steps: S1, stirring and mixing the carrier resin, silicone elastomer microparticles grafted with polar groups, a bridging agent, and a noise reduction auxiliary agent, adding color paste, epoxy soybean oil acrylate, and glucomannan, stirring, dispersing, and degassing to obtain a surface treatment agent; S2, cleaning the artificial leather base material; S3, roller-coating the surface treatment agent on the surface of the artificial leather base material, drying, heat-treating, and cooling to obtain the wear-resistant and noise-reducing artificial leather material.

[0024] By adopting the above technical solution, the preparation method adopted in this application has a simple process and high production efficiency. Through stirring, dispersing and degassing treatment, the surface treatment agent components are ensured to be evenly dispersed, reducing the agglomeration and stratification phenomena that may occur in traditional processes, and improving the wear resistance and noise reduction effect of the coating. The prepared artificial leather material has excellent wear resistance and can effectively reduce friction noise.

[0025] Optionally, in step S3, the heat treatment temperature is 120-150° C., and the heat treatment time is 0.5-2 h.

[0026] By adopting the above technical solution, the heat treatment temperature and heat treatment time of the present application can make the coating stronger, improve wear resistance, and also help the noise reduction additive in the coating to better play its role and reduce friction noise.

[0027] In summary, the present invention includes at least one of the following beneficial technical effects: 1. The present application adopts specific raw materials and proportions, and the artificial leather material produced has excellent wear resistance and can effectively reduce friction noise.

[0028] 2. This application adds a carrier resin with excellent wear resistance and silicone elastomer micron particles with excellent noise reduction performance to optimize the microstructure of the coating, reduce the friction noise between materials, and enhance the user's auditory experience.

[0029] 3. The preparation method adopted in this application has a simple process and high production efficiency, reduces the agglomeration and stratification phenomena that may occur in traditional processes, and improves the wear resistance and noise reduction effect of the coating. DETAILED DESCRIPTION

[0030] The present application is further described in detail below with reference to the embodiments.

[0031] The present application designs an abrasion-resistant and noise-reducing artificial leather material, comprising an artificial leather base material and a surface treatment agent coated on the surface of the artificial leather base material; the surface treatment agent comprises 90 to 110 parts of a carrier resin, 1 to 15 parts of organic silicone elastomer micron particles grafted with polar groups, 5 to 10 parts of a bridging agent, 1 to 10 parts of a noise reduction aid, 5 to 10 parts of a color paste, 5 to 10 parts of epoxy soybean oil acrylate, and 0.5 to 1 part of glucomannan.

[0032] The wear-resistant and noise-reducing artificial leather material of the present application is prepared by the following method, comprising the following steps: S1, mixing the carrier resin, the organosilicon elastomer microparticles grafted with polar groups, the bridging agent, and the noise reduction agent, adding color paste, epoxy soybean oil acrylate, and glucomannan, stirring, dispersing, and degassing to obtain a surface treatment agent; S2, cleaning the artificial leather base material; S3, roller-coating the surface treatment agent on the surface of the artificial leather base material, drying, heat-treating, and cooling to obtain the wear-resistant and noise-reducing artificial leather material.

[0033] The applicant has designed the technical solution of the present application to solve the problems of insufficient wear resistance and high friction noise of existing artificial leather materials.

[0034] The raw materials used in this application are as follows: Polyurethane resin: CAS: 9009-54-5.

[0035] Polyester resin: CAS: 109-16-0.

[0036] Sodium dodecyl sulfate: CAS: 151-21-3.

[0037] Polymethylvinylsiloxane: CAS: 68037-87-6.

[0038] 3-Aminopropyltriethoxysilane: CAS: 919-30-2.

[0039] Isocyanate: CAS: 75-13-8.

[0040] Titanate: CAS: 5593-70-4.

[0041] Polyethylene wax: CAS: 9002-88-4.

[0042] Dimethylpolysiloxane: CAS: 8050-81-5.

[0043] Epoxidized soybean oil acrylate: Hubei Chengfeng Chemical Co., Ltd., purity: 99%.

[0044] Glucomannan: CAS: 11078-31-2. Specific embodiments

[0045] The preparation method of the organic silicon elastomer microparticles grafted with polar groups used in Examples 1 to 3 is as follows: 1 g of sodium dodecyl sulfate is dissolved in 100 ml of deionized water, heated to 70° C., and dissolved to obtain a sodium dodecyl sulfate solution; 10 g of polymethylvinylsiloxane is dissolved in 20 ml of ethanol, stirred to obtain a polymethylvinylsiloxane solution; the polymethylvinylsiloxane solution is added dropwise to the sodium dodecyl sulfate solution, and stirred for 30 minutes using a high-speed stirrer to obtain an emulsion; 2 g of 3-aminopropyltriethoxysilane is added to the emulsion, continued to stir, and reacted at room temperature for 12 hours; dilute hydrochloric acid is added to adjust the pH value to 5; 10 ml of calcium chloride solution (concentration of 0.1 mol / L) is added to the emulsion after the reaction, stirred for 30 minutes, washed, separated, dried, and sieved to obtain organic silicon elastomer microparticles grafted with hydroxyl groups, with an average particle size of 5 μm.

[0046] Examples 1 to 3 Example 1 The present embodiment provides a wear-resistant and noise-reducing artificial leather material, comprising an artificial leather base material and a surface treatment agent coated on the surface of the artificial leather base material; the surface treatment agent comprises 110 parts of a carrier resin, 1 part of organic silicone elastomer micron particles grafted with hydroxyl groups, 10 parts of a bridging agent, 1 part of a noise reduction auxiliary agent, 10 parts of a color paste, 5 parts of epoxy soybean oil acrylate, and 0.5 parts of glucomannan; The carrier resin is polyurethane resin; the bridging agent is isocyanate; the noise reduction agent is polyethylene wax; the average particle size of the noise reduction agent is 5 μm; The preparation method comprises the following steps: S1. Mixing a carrier resin, silicone elastomer microparticles grafted with hydroxyl groups, a bridging agent, and a noise reduction agent, adding a color paste, epoxy soybean oil acrylate, and glucomannan, stirring, dispersing, and degassing to obtain a surface treatment agent; S2, cleaning the artificial leather base material; S3, coating the surface treatment agent on the surface of the artificial leather base material with a roller, drying, heat treating at 135° C. for 1.2 h, and cooling to obtain a wear-resistant and noise-reducing artificial leather material.

[0047] Example 2 The present embodiment provides a wear-resistant and noise-reducing artificial leather material, comprising an artificial leather base material and a surface treatment agent coated on the surface of the artificial leather base material; the surface treatment agent comprises 100 parts of a carrier resin, 8 parts of organic silicone elastomer microparticles grafted with hydroxyl groups, 8 parts of a bridging agent, 5 parts of a noise reduction aid, 8 parts of a color paste, 8 parts of epoxy soybean oil acrylate, and 0.8 parts of glucomannan; The carrier resin is polyurethane resin; the bridging agent is isocyanate; the noise reduction agent is polyethylene wax; the average particle size of the noise reduction agent is 5 μm; The preparation method comprises the following steps: S1. Mixing a carrier resin, silicone elastomer microparticles grafted with hydroxyl groups, a bridging agent, and a noise reduction agent, adding a color paste, epoxy soybean oil acrylate, and glucomannan, stirring, dispersing, and degassing to obtain a surface treatment agent; S2, cleaning the artificial leather base material; S3, coating the surface treatment agent on the surface of the artificial leather base material with a roller, drying, heat treating at 135° C. for 1.2 h, and cooling to obtain a wear-resistant and noise-reducing artificial leather material.

[0048] Example 3 The present embodiment provides a wear-resistant and noise-reducing artificial leather material, comprising an artificial leather base material and a surface treatment agent coated on the surface of the artificial leather base material; the surface treatment agent comprises 90 parts of a carrier resin, 15 parts of organic silicone elastomer microparticles grafted with hydroxyl groups, 5 parts of a bridging agent, 10 parts of a noise reduction aid, 5 parts of a color paste, 10 parts of epoxy soybean oil acrylate, and 1 part of glucomannan; The carrier resin is polyurethane resin; the bridging agent is isocyanate; the noise reduction agent is polyethylene wax; the average particle size of the noise reduction agent is 5 μm; The preparation method comprises the following steps: S1. Mixing a carrier resin, silicone elastomer microparticles grafted with hydroxyl groups, a bridging agent, and a noise reduction agent, adding a color paste, epoxy soybean oil acrylate, and glucomannan, stirring, dispersing, and degassing to obtain a surface treatment agent; S2, cleaning the artificial leather base material; S3, coating the surface treatment agent on the surface of the artificial leather base material with a roller, drying, heat treating at 135° C. for 1.2 h, and cooling to obtain a wear-resistant and noise-reducing artificial leather material.

[0049] Comparative Examples 1 to 5 Comparative Example 1 The difference between Comparative Example 1 and Example 2 is that the surface treatment agent of Comparative Example 1 does not contain any organosilicon elastomer microparticles grafted with hydroxyl groups.

[0050] Comparative Example 2 The difference between Comparative Example 2 and Example 2 is that in Comparative Example 2, the hydroxyl-grafted silicone elastomer microparticles are replaced with ordinary silicone elastomer microparticles.

[0051] Comparative Example 3 The difference between Comparative Example 3 and Example 2 is that epoxy soybean oil acrylate and glucomannan are not added to the surface treatment agent of Comparative Example 3.

[0052] Comparative Example 4 The difference between Comparative Example 4 and Example 2 is that epoxy soybean oil acrylate is not added to the surface treatment agent of Comparative Example 4.

[0053] Comparative Example 5 The difference between Comparative Example 5 and Example 2 is that no glucomannan is added to the surface treatment agent in Comparative Example 5.

[0054] Experimental testing Test items and test methods Abrasion resistance test: The abrasion resistance of the artificial leather material is tested according to GB / T 2726-2005 “Determination of abrasion resistance of leather by physical and mechanical tests”.

[0055] Noise reduction test: The noise resistance test of the artificial leather material is carried out according to the German automotive industry standard VDA 230-206; The specific test method is as follows: cut two sheets from artificial leather, namely sheet A and sheet B, and fix sheet A to the instrument described in Part 3 of VDA230-206 as a fixed sheet. Install sheet B on the moving head of the instrument. Press sheet B against sheet A, and operate the moving head to move sheet B on sheet A. Adjust the pressure of sheet B against sheet A so that the pressure is 10N and 40N respectively. For each adjusted pressure, adjust the speed at which sheet B moves on sheet A, and perform noise tests at speeds of 1mm / s and 4mm / s respectively. Record the noise level value for each test and take the average value. The lower the noise level value, the better the noise reduction effect of the artificial leather material.

[0056] The artificial leather materials prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were tested for wear resistance and noise level values. The test results are shown in Table 1.

[0057] Table 1 From the test results in Table 1, it can be seen that the artificial leather materials prepared in Examples 1 to 3 have excellent wear resistance and low noise level values, and can effectively reduce friction noise.

[0058] In the surface treatment agent of Comparative Example 1, no organosilicon elastomer micron particles grafted with hydroxyl groups were added, and the wear resistance of the prepared artificial leather material was significantly reduced, the friction noise was large, and the noise reduction effect was poor.

[0059] In Comparative Example 2, the organosilicon elastomer microparticles grafted with hydroxyl groups were replaced with ordinary organosilicon elastomer microparticles, and the wear resistance and noise reduction effects of the prepared artificial leather material were reduced.

[0060] The wear resistance and noise reduction effects of the artificial leather materials prepared in Comparative Examples 3 to 5 are inferior to those in Example 2.

[0061] Embodiments 4 to 12 Example 4 The difference between Example 4 and Example 2 is that the carrier resin in the surface treatment agent of Example 4 is a polyester resin.

[0062] Example 5 The difference between Example 5 and Example 2 is that in Example 5, the organosilicon elastomer microparticles grafted with hydroxyl groups account for 3% of the total amount of the surface treatment agent.

[0063] Example 6 The difference between Example 6 and Example 2 is that in Example 6, the organosilicon elastomer microparticles grafted with hydroxyl groups account for 7% of the total amount of the surface treatment agent.

[0064] Example 7 The difference between Example 7 and Example 2 is that the bridging agent in the surface treatment agent of Example 7 is titanate.

[0065] Example 8 The difference between Example 8 and Example 2 is that the noise reduction agent in the surface treatment agent of Example 8 is dimethyl polysiloxane.

[0066] Example 9 The difference between Example 9 and Example 2 is that in Example 9, the average particle size of the noise reduction agent is 0.1 μm.

[0067] Example 10 The difference between Example 10 and Example 2 is that in Example 10, the average particle size of the noise reduction agent is 10 μm.

[0068] Embodiment 11 The difference between Example 11 and Example 2 is that in the surface treatment agent of Example 11, the weight ratio of epoxy soybean oil acrylate and glucomannan is 8:1, and the total weight of epoxy soybean oil acrylate and glucomannan is 8.8.

[0069] Example 12 The difference between Example 12 and Example 2 is that in the surface treatment agent of Example 12, the weight ratio of epoxy soybean oil acrylate and glucomannan is 12:1, and the total weight of epoxy soybean oil acrylate and glucomannan is 8.8.

[0070] The artificial leather materials prepared in Examples 4 to 12 were tested for wear resistance and noise level. The test results are shown in Table 2.

[0071] Table 2 From the test results in Table 2, it can be seen that the wear resistance and noise reduction effect of the artificial leather material prepared in Example 4 are similar to those in Example 2.

[0072] The difference between Example 5 and Example 6 and Example 2 is that the proportion of the organosilicon elastomer microparticles grafted with hydroxyl groups to the total amount of the surface treatment agent is different, and the artificial leather material prepared in Example 2 has the best wear resistance.

[0073] The wear resistance and noise reduction effect of the artificial leather materials prepared in Examples 7 and 8 are similar to those in Example 2.

[0074] The difference between Example 9 and Example 10 and Example 2 is that the average particle sizes of the noise reduction additives are different. Among them, the artificial leather material prepared in Example 2 has the best wear resistance and noise reduction effect.

[0075] The difference between Example 11 and Example 12 and Example 2 is that the weight ratios of epoxy soybean oil acrylate and glucomannan are different. Among them, the artificial leather material prepared in Example 2 has the best wear resistance and noise reduction effect.

[0076] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A wear-resistant and noise-reducing artificial leather material, characterized in that: The invention comprises an artificial leather base material and a surface treatment agent coated on the surface of the artificial leather base material; the surface treatment agent comprises 90-110 parts of a carrier resin, 1-15 parts of organic silicon elastomer micron particles grafted with polar groups, 5-10 parts of a bridging agent, 1-10 parts of a noise reduction auxiliary agent, 5-10 parts of a color paste, 5-10 parts of epoxy soybean oil acrylate, and 0.5-1 part of glucomannan.

2. The wear-resistant and noise-reducing artificial leather material according to claim 1, characterized in that: The carrier resin is selected from one of polyurethane resin, acrylic resin and polyester resin.

3. The wear-resistant and noise-reducing artificial leather material according to claim 1, characterized in that: In the organic silicon elastomer micronized particles grafted with polar groups, the polar groups are one of hydroxyl, amino and carboxyl groups.

4. The wear-resistant and noise-reducing artificial leather material according to claim 1, characterized in that: The organosilicon elastomer microparticles grafted with polar groups account for 3-7% of the total amount of the surface treatment agent.

5. The wear-resistant and noise-reducing artificial leather material according to claim 1, characterized in that: The bridging agent is selected from at least one of isocyanate, epoxy resin and titanate.

6. The wear-resistant and noise-reducing artificial leather material according to claim 1, characterized in that: The noise reduction agent is selected from at least one of polyethylene wax, dimethyl polysiloxane and polytetrafluoroethylene.

7. The wear-resistant and noise-reducing artificial leather material according to claim 1, characterized in that: The average particle size of the noise reduction agent is 0.1-10 μm.

8. The wear-resistant and noise-reducing artificial leather material according to claim 1, characterized in that: The weight ratio of the epoxy soybean oil acrylate to glucomannan is 8-12:

1.

9. A method for preparing the wear-resistant and noise-reducing artificial leather material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, mixing the carrier resin, the organosilicon elastomer microparticles grafted with polar groups, the bridging agent, and the noise reduction agent, adding color paste, epoxy soybean oil acrylate, and glucomannan, stirring, dispersing, and degassing to obtain a surface treatment agent; S2, cleaning the artificial leather base material; S3, roller-coating the surface treatment agent on the surface of the artificial leather base material, drying, heat-treating, and cooling to obtain the wear-resistant and noise-reducing artificial leather material.

10. The method for preparing the wear-resistant and noise-reducing artificial leather material according to claim 9, characterized in that: In step S3, the heat treatment temperature is 120-150° C., and the heat treatment time is 0.5-2 h.