Photoresist coating method suitable for high-step substrate

By spraying diluent on a high-step silicon carbide substrate and adjusting the rotation speed, the photoresist viscosity is reduced, and the problems of poor uniformity and abnormal appearance during photoresist coating are solved, and the uniform coverage of photoresist is achieved. High resolution process improves the fluidity and coating quality of photoresist.

CN119045285APending Publication Date: 2024-11-29HANGZHOU HESHENG MICROELECTRONICS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411456729.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

When applying photoresist on high-step silicon carbide substrates, poor uniformity and abnormal appearance are prone to occur, resulting in the impact of subsequent processes. The existing methods solve the problem by increasing the thickness of the photoresist, but the uniformity of the uniformity is reduced and it cannot be achieved High resolution lithography process.

Method used

By spraying diluent on the wafer stage and adjusting the rotation speed, the diluent remains on the substrate surface, reducing the viscosity of the photoresist and improving fluidity, the method of retaining diluent on the substrate surface is used to achieve immediate photoresist Dilution improves the fluidity and coating quality of the photoresist.

Benefits of technology

The uniform coverage of photoresist on the high-step substrate is achieved, the adhesion and utilization of photoresist is improved, the uniform thickness of the resist film pattern is ensured, and the resolution and coating quality of the photolithography process are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119045285A_ABST
    Figure CN119045285A_ABST
Patent Text Reader

Abstract

The invention discloses a photoresist coating method suitable for a high-step substrate, which comprises the following steps: S1, placing a substrate to be coated with photoresist on a wafer carrying table, keeping the wafer carrying table at a first rotating speed v1 which is greater than or equal to 1,500 revolutions per minute, and spraying a diluent on the surface of the substrate for t1; s2, the rotating speed of the wafer carrier is adjusted to a second rotating speed v2, the diluent continues to be sprayed, the continuous rotating time of the carrier is t2, the ratio of the volume of the sprayed diluent to the volume of the photoresist sprayed in the step S3 is 1: 1-1: 5, and v2 is smaller than 500 revolutions per minute; s3, the rotating speed v2 is kept, photoresist is sprayed to the surface of the substrate in the step S2, the wafer carrying table is kept at the third rotating speed v3 after spraying, the photoresist is made to be self-leveled, and v2 is smaller than v3; and S4, adjusting the rotating speed of the wafer stage to a process preset rotating speed v4, and obtaining a photoresist layer with a preset thickness on the surface of the substrate. According to the invention, the mobility of the photoresist is improved through the diluent sprayed on the substrate, so that the photoresist layer is uniformly thickened, and a high-resolution photoetching process is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor manufacturing, and in particular to a photoresist coating method suitable for high-step substrates. Background Art

[0002] Photolithography is one of the key processes in semiconductor manufacturing. The photolithography process is to transfer the pre-designed pattern to the photoresist on the surface of the substrate. The main steps of the photolithography process include coating, exposure, and development. Among them, the purpose of the coating process is to form a uniform photoresist layer on the surface of the substrate.

[0003] For silicon carbide wafer substrates, after some special processes, uneven graphic steps will be formed on the surface. When applying photoresist on such a surface, defects such as poor coating and abnormal appearance are likely to occur, thus affecting subsequent processes. At present, when applying photoresist on silicon carbide substrates with high step structures, the unevenness of the coating surface is usually reduced by increasing the thickness of the photoresist. However, if the photoresist is applied too thickly, it is easy to reduce the uniformity of coating and fail to achieve high-resolution lithography. Summary of the invention

[0004] One purpose of the present application is to provide a method for coating a photoresist suitable for a high-step substrate, which is conducive to obtaining a photoresist layer with a smooth surface.

[0005] To achieve the above objectives, the technical solution adopted in this application is: a photoresist coating method suitable for a high-step substrate, comprising the following steps:

[0006] S1. Placing the substrate to be coated with photoresist on a wafer stage, the wafer stage maintains a first rotation speed v1, v1 ≥ 1500 rpm, spraying a diluent onto the surface of the substrate for a spraying time of t1, so that the surface of the substrate is wetted;

[0007] S2. The rotation speed of the wafer stage is adjusted to a second rotation speed v2, and the diluent is continued to be sprayed. The wafer stage continues to rotate for a time t2, and the ratio of the volume of the sprayed diluent to the volume of the photoresist sprayed in step S3 is 1:1 to 1:5, and v2 is less than 500 rpm;

[0008] S3. The wafer stage maintains a rotation speed of v2, sprays photoresist onto the surface of the substrate in step S2, and after spraying, the wafer stage maintains a third rotation speed v3 to make the photoresist self-leveling, v2<v3;

[0009] S4. Adjust the rotation speed of the wafer stage to a process preset rotation speed v4 to obtain a photoresist layer of preset thickness on the surface of the substrate.

[0010] As a preference, the ratio of the volume of the diluent sprayed in step S2 to the volume of the photoresist sprayed in step S3 is 1:1 to 1:3.

[0011] As a preference, the ratio of the volume of the diluent sprayed in step S2 to the volume of the photoresist sprayed in step S3 is 1:2.

[0012] As a preferred embodiment, t2≤3s.

[0013] As a preferred embodiment, v2 is 100-200 rpm, and t2≤3s.

[0014] As a preferred embodiment, t1≤5s.

[0015] As a preferred embodiment, v1 is 1500-2500 rpm, and t1≤3s.

[0016] As a preferred embodiment, v3 is 700-1000 rpm, and t3≤5s.

[0017] As a preference, in any of the above-mentioned photoresist coating methods, in step S3, the viscosity of the sprayed photoresist is not less than 29 cp.

[0018] As a preference, in any of the photoresist coating methods, the diluent is an inactive diluent, comprising one or more combinations of the following: propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate.

[0019] Compared with the prior art, the beneficial effects of this application are:

[0020] (1) In the present application, the diluent wets the substrate in advance, which helps to improve the adhesion of the photoresist during subsequent coating, making it difficult for the photoresist to be thrown out of the substrate, thereby improving the utilization rate of the photoresist.

[0021] (2) In step S2 of the present application, by reducing the rotation speed, most of the diluent remains on the surface of the substrate. After the subsequent spraying of the photoresist, the viscosity of the photoresist can be reduced, the fluidity of the photoresist can be improved, and the photoresist can be more evenly covered on the surface of the substrate during the coating process, ensuring the uniform thickening of the anti-etching film pattern.

[0022] (3) The present application adopts the method of retaining the diluent on the substrate surface to achieve immediate dilution of the photoresist, which helps to improve the photoresist dilution efficiency and the fluidity of the photoresist, thereby improving the photoresist coating quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 4 is a process flow chart of photoresist thinner coating in an embodiment of the present invention.

[0024] Figure 2Schematic diagram of a high-step silicon carbide substrate with an undulating surface in an embodiment of the present invention.

[0025] Figure 3 This is a schematic diagram of the large height difference of the photoresist thickness on the surface of a high-step silicon carbide substrate after coating using the existing photoresist spraying method.

[0026] Figure 4 Schematic diagram of the self-leveling coating of diluted photoresist in an embodiment of the present invention.

[0027] Figure 5 Schematic diagram of the photoresist film after coating in an embodiment of the present invention.

[0028] In the figure: 100, substrate; 200, photoresist layer; 200A, existing photoresist layer. DETAILED DESCRIPTION

[0029] Below, the present application is further described in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.

[0030] In the description of the present application, it should be noted that directional words, such as the terms "center", "lateral", "longitudinal", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc., indicating directions and positional relationships are based on the directions or positional relationships shown in the accompanying drawings, which are only for the convenience of narrating the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and cannot be understood as limiting the specific scope of protection of the present application.

[0031] It should be noted that the terms "first", "second", etc. in the description and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence.

[0032] The terms "including" and "having" and any variations thereof in the specification and claims of this application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or apparatuses.

[0033] The method for solving the abnormal coating of high-step photoresist in the prior art is usually to increase the thickness of the photoresist layer to reduce the unevenness of the coating surface, but too thick a photoresist layer will reduce the uniformity of the coating and fail to achieve a high-resolution photolithography process. Therefore, the inventors disclose a novel photoresist coating method, which increases the fluidity of the subsequently sprayed photoresist by spraying a diluent on a wafer carrier and leaving a certain amount of diluent, so that the photoresist can be evenly covered on the substrate surface during the coating process, thereby improving the resolution of the photolithography process.

[0034] The present application discloses a photoresist coating method suitable for a high-step substrate, comprising the following steps:

[0035] S1. Place the substrate 100 to be coated with photoresist on a wafer stage, maintain the wafer stage at a first rotation speed v1, v1 ≥ 1500 rpm, spray the diluent onto the surface of the substrate 100 for a spraying time of t1, so that the surface of the substrate 100 is wetted;

[0036] S2. The rotation speed of the wafer stage is adjusted to a second rotation speed v2, and the diluent is continued to be sprayed. The wafer stage continues to rotate for a time t2, and the ratio of the volume of the sprayed diluent to the volume of the photoresist sprayed in step S3 is 1:1 to 1:5, and v2 is less than 500 rpm;

[0037] S3. The wafer stage is maintained at a rotation speed v2, and the photoresist is sprayed onto the surface of the substrate 100 in step S2. After spraying, the wafer stage is maintained at a third rotation speed v3 to make the photoresist self-leveling, v2<v3;

[0038] S4. Adjust the rotation speed of the wafer stage to a process preset rotation speed v4 to obtain a photoresist layer 200 of a preset thickness on the surface of the substrate 100.

[0039] Specifically, in step S1 , the entire surface of the substrate 100 is wetted by the diluent. After the substrate 100 is wetted by the diluent, the surface tension of the substrate 100 can be reduced, so that the photoresist can be spread evenly on the substrate 100 more easily.

[0040] Specifically, in step S2, by reducing the wafer stage rotation speed, most of the continuously sprayed diluent can remain on the surface of the substrate 100. If the volume of the diluent remaining on the surface of the substrate 100 after spraying the diluent is too small, it will not fully dilute the photoresist, and if it is too large, the viscosity of the photoresist will be reduced, and the drying time of the photoresist will be prolonged, thereby affecting the production efficiency. Therefore, the ratio of the volume of the sprayed diluent in step S2 to the volume of the photoresist sprayed in step S3 is 1:1 to 1:5, which can ensure that the diluent on the surface of the substrate 100 effectively dilutes the photoresist subsequently coated on the surface of the substrate 100, reduces the viscosity of the photoresist, improves the fluidity of the photoresist, and forms a uniform photoresist layer 200.

[0041] In some embodiments, the ratio of the volume of the diluent sprayed in step S2 to the volume of the photoresist sprayed in step S3 ranges from 1:1 to 1:3.

[0042] In some embodiments, the ratio of the volume of the diluent sprayed in step S2 to the volume of the photoresist sprayed in step S3 is 1:2.

[0043] Specifically, in step S2, if the rotation speed of the spraying diluent is too high, it is easy for the diluent to be thrown around the substrate 100 during the spraying process. If the rotation time of the wafer carrier is too long, it is easy for the diluent that has remained on the surface of the substrate 100 to be thrown out of the surface of the substrate 100, so that the amount of diluent retained on the surface of the substrate 100 is too small, affecting the dilution of the photoresist in the subsequent step S3. Therefore, the second rotation speed of the spraying diluent is reduced to v2<500 rpm, and the rotation time is t2≤3s, which can ensure that the sprayed diluent remains on the surface of the substrate 100 and effectively dilutes the photoresist sprayed in the subsequent step S3.

[0044] In some embodiments, the second rotation speed v2 maintained by spraying the diluent in step S2 is 100 to 200 rpm.

[0045] Specifically, in step S1, when the diluent is sprayed to wet the surface of the substrate 100, the first rotation speed of the wafer stage is v1 ≥ 1500 rpm, and the rotation time of the wafer stage is t1 ≤ 5s. The higher rotation speed can ensure that the diluent is sprayed to the center and edge of the surface of the substrate 100, so that the surface of the substrate 100 is fully wetted, and the adhesion of the surface of the substrate 100 is improved, so that most of the diluent that continues to be sprayed can be retained on the surface of the substrate 100, reducing the waste of subsequent diluent. In addition, spraying the diluent at a higher rotation speed can also shorten the rotation time of the wafer stage, thereby quickly completing the wetting of the surface of the substrate 100 and improving the efficiency of photoresist coating.

[0046] In some embodiments, in step S1 , the first rotation speed v1 of spraying the diluent to wet the surface of the substrate 100 is 1500-2500 rpm, and t1≤3s.

[0047] Specifically, in step S3, when spraying photoresist onto the surface of the substrate 100 in step S2, the rotation speed of the wafer carrier is increased and maintained at a third rotation speed v3 of 700 to 1000 rpm, t3≤5s, to ensure that the photoresist can achieve self-leveling on the surface of the substrate 100 and form a uniform photoresist layer 200, thereby improving the resolution of the photolithography process.

[0048] Specifically, in any of the photoresist coating methods described, the viscosity of the photoresist sprayed in step S3 is not less than 29cp, because the low-viscosity photoresist will have stronger fluidity on the surface of the substrate 100 after being diluted by the diluent, resulting in uneven thickness of the photoresist layer 200 after coating, with the edge being thick and the center being thin, affecting the accuracy of subsequent processes.

[0049] In certain embodiments, the process adopted when photoresist is coated is to mix the diluent in the photoresist in advance, but mixing the diluent in advance may affect the stability of the photoresist. Because photoresist usually has a certain shelf life and storage condition requirements, after adding the diluent, its chemical property may change, thereby causing the shelf life to be shortened or the storage conditions to be more harsh. In addition, the mixed photoresist may be more sensitive to environmental factors such as temperature, humidity, etc., and small environmental changes may cause the larger fluctuation of the photoresist performance, thereby affecting the stability of the coating quality. Therefore, the application proposes a novel photoresist coating method, by wetting the substrate 100 in advance, and making the substrate 100 residual part of the diluent, completing the dilution of the photoresist while the photoresist is sprayed, improving the fluidity of the photoresist, enabling it to fill the high step, and ensuring the coating uniformity of the photoresist.

[0050] In some embodiments, the diluent is an inactive diluent that does not participate in the chemical reaction of the photoresist and does not change the properties of the photoresist. The diluent type includes a combination of one or more of the following: propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate.

[0051] Specifically, the photoresist coating method of the present invention is implemented in the following steps:

[0052] S1. Place the substrate 100 to be coated with photoresist on a wafer stage, maintain the first rotation speed v1 of the wafer stage at 1500 to 2500 rpm, spray the diluent propylene glycol monomethyl ether on the surface of the substrate 100, and rotate the wafer stage for a time of t1≤3s, so that most of the surface of the substrate 100 is wetted;

[0053] S2. According to the ratio of the volume of the sprayed diluent to the volume of the photoresist sprayed in step S3 of 1:1 to 1:5, the volume of the diluent to be sprayed is calculated in advance, the rotation speed of the wafer carrier is adjusted to a second rotation speed v2 of 100 to 200 rpm, and then the calculated diluent propylene glycol monomethyl ether is continued to be sprayed onto the surface of the substrate 100, and the wafer carrier continues to rotate for a time of t2≤3s, so that the diluent remains on the surface of the substrate 100;

[0054] S3. According to the ratio of the volume of the sprayed diluent to the volume of the photoresist sprayed in step S3 of 1:1 to 1:5, the volume of the photoresist to be sprayed is calculated in advance, the wafer stage continues to maintain the second speed v2 of 100 to 200 rpm, and the calculated photoresist is sprayed on the surface of the substrate 100. After the photoresist is sprayed, the wafer stage speed is increased, and the third speed v3 is maintained at 700 to 1000 rpm. The rotation time of the wafer stage is t3 ≤ 5s, so that the photoresist is self-leveling;

[0055] S4. Adjust the rotation speed of the wafer stage to a preset rotation speed, and obtain a photoresist layer 200 of a preset thickness on the surface of the substrate 100 .

[0056] It is worth mentioning that the photoresist coating method of the present invention is applicable to any substrate, such as a high-step silicon carbide substrate, a single crystal silicon substrate, a polycrystalline silicon substrate, a germanium silicon substrate, a sapphire substrate or other semiconductor substrates that require photolithography.

[0057] like Figure 3 As shown, the thickness of the existing photoresist layer 200A formed on the surface of the high-step silicon carbide substrate 100 after coating using the existing photoresist spraying process has a large height difference. The photoresist coating method in the present application uses the diluent remaining on the surface of the substrate 100 to increase the fluidity of the photoresist, and then adjusts the rotation speed of the carrier when spraying the diluent and photoresist, so as to achieve the purpose of self-leveling of the photoresist, fully fill the surface steps, reduce the surface height difference, solve the problems of poor coating and abnormal appearance during the coating process, and improve the photolithography resolution.

[0058] The following will be combined Figure 1 , Figure 2 , Figure 4 and Figure 5 A photoresist coating method for a high-step silicon carbide substrate 100 is further described in detail in the specific embodiment of the invention:

[0059] Example 1

[0060] (1) If Figure 2 As shown, a 6-inch high-step silicon carbide substrate 100 with an undulating surface is provided. First, the 6-inch high-step silicon carbide substrate 100 to be coated with photoresist is placed on a wafer stage, and then the wafer stage is kept rotating at a speed of 2000 rpm to start rotating. During the rotation process, a diluent propylene glycol monomethyl ether is sprayed on the surface of the high-step silicon carbide substrate 100. The diluent is sprayed for 3 seconds while the wafer stage is kept rotating, so that most of the surface of the high-step silicon carbide substrate 100 is wetted;

[0061] (2) Reduce the rotation speed of the wafer stage to 200 rpm, spray 2 ml of propylene glycol monomethyl ether as a diluent, and keep the wafer stage rotating for 2 seconds, so that the residual diluent on the surface of the substrate 100 is about 2 ml;

[0062] (3) Maintain the wafer stage at a rotation speed of 200 rpm, spray 2 ml of photoresist onto the surface of the high-step silicon carbide substrate 100, increase the wafer stage rotation speed to 800 rpm after the photoresist spraying is completed, and keep the wafer stage rotating for 5 seconds to allow the photoresist to achieve self-leveling on the high-step silicon carbide substrate 100, such as Figure 4 As shown;

[0063] (4) After the photoresist is self-leveled, the rotation speed of the wafer stage is further increased to 2500 rpm, and the wafer stage is kept rotating at 2500 rpm for 30 seconds to obtain a photoresist layer 200 with a thickness of 2 μm on the surface of the high-step silicon carbide substrate 100. Figure 5 shown.

[0064] Example 2

[0065] The difference between Example 2 and Example 1 is that in step (2), the rotation speed of the wafer carrier is 150 rpm, and 4 ml of propylene glycol monomethyl ether is sprayed as the diluent (the residual diluent on the wafer surface is about 4 ml); in step (3), the rotation speed of the wafer carrier is maintained at 150 rpm, 8 ml of photoresist is sprayed onto the surface of the high-step silicon carbide substrate 100, and the rotation speed of the wafer carrier is increased to 900 rpm after spraying the photoresist.

[0066] Example 3

[0067] The difference between Example 3 and Example 1 is that in step (2), the rotation speed of the wafer carrier is 100 rpm, and 6 ml of propylene glycol monomethyl ether is sprayed as the diluent (about 6 ml of the diluent remains on the wafer surface); in step (3), the rotation speed of the wafer carrier is maintained at 100 rpm, 8 ml of photoresist is sprayed onto the surface of the high-step silicon carbide substrate 100, and the rotation speed of the wafer carrier is increased to 1000 rpm after spraying the photoresist.

[0068] Comparative Example 1

[0069] The difference between Comparative Example 1 and Example 2 is that in Comparative Example 1, the rotation speed of the wafer carrier in step (2) is still maintained at 150 rpm, but the spraying of the diluent is cancelled.

[0070] Comparative Example 2

[0071] The difference between Comparative Example 2 and Example 2 is that the rotation speed of the wafer carrier in step (2) is 800 rpm.

[0072] Comparative Example 3

[0073] The difference between Comparative Example 3 and Example 2 is that the rotation speed of the wafer carrier in step (3) is 1500 rpm.

[0074] Comparative Example 4

[0075] The difference between Comparative Example 4 and Example 2 is that the rotation speed of the wafer carrier in step (3) is 500 rpm.

[0076] Comparative Example 5

[0077] The difference between Comparative Example 5 and Example 2 is that the ratio of the amount of diluent used in step (2) to the amount of photoresist used in step (3) is 1:0.8.

[0078] Comparative Example 6

[0079] The difference between Comparative Example 6 and Example 2 is that the ratio of the amount of diluent used in step (2) to the amount of photoresist used in step (3) is 1:6.

[0080] Comparative Example 7

[0081] The difference between Comparative Example 7 and Example 2 is that Comparative Example 8 eliminates the step (1) of spraying the diluent to wet the surface of the substrate 100 .

[0082] It is worth mentioning that the above-mentioned photoresist coating process is applicable to all methods of changing the fluidity of the photoresist to make the photoresist self-leveling and filling holes without affecting the function of the photoresist.

[0083] The semiconductor device manufactured by the silicon carbide substrate in the above embodiment and comparative example is a silicon carbide MOSFET device. Except for the different photoresist coating process, the other semiconductor device manufacturing steps are the same, and the final semiconductor device yield is shown in Table 1. It is worth mentioning that the coating quality of the photoresist will mainly cause defects such as pattern missing and pattern abnormality in the subsequent process, and these defects will eventually reduce the yield of the semiconductor device. This application uses the yield data of the semiconductor device to illustrate the impact of the photoresist coating process on the final device performance. Table 1

[0084] Comparing the data of the above-mentioned Example 2 and Comparative Example 1, when the substrate is wetted, step (2) lacks the process of spraying a diluent on the substrate surface to dilute the photoresist, and the photoresist is directly sprayed on the substrate surface. The photoresist cannot be self-leveled, and the high step structure on the substrate surface will cause uneven or missing photoresist spin coating, thereby reducing the yield of the subsequently manufactured semiconductor devices.

[0085] Comparing the data of the above-mentioned Example 2 and Comparative Example 2, when the rotation speed of the spraying diluent in step (2) is too high, most of the diluent is thrown out of the substrate surface, so that too little diluent is left on the substrate surface, and it is difficult for the photoresist to form a uniform covering layer on the substrate, resulting in uneven dissolution of the photoresist during the development process, pattern loss, and the yield of the semiconductor device is only 81%.

[0086] Comparing the data of the above-mentioned Example 2 with those of Comparative Examples 3 and 4, during the photoresist spraying process in step (3), a rotation speed of the wafer carrier that is too high or too low is not conducive to the filling of high steps after the photoresist is self-leveled, resulting in uneven dissolution of the photoresist during the development of the semiconductor device, abnormal patterns, and thus affecting the yield of the semiconductor device.

[0087] Comparing the data of Example 2 and Comparative Examples 5 and 6, if the ratio of the amount of diluent used in step (2) to the amount of photoresist used in step (3) is too low or too high, stripes or a photoresist layer with localized uneven thickness may be easily formed, thereby affecting the pattern after development and reducing the yield of the semiconductor device.

[0088] Comparing the data of the above-mentioned Example 2 and Comparative Example 7, when the photoresist coating lacks step (1) of wetting the substrate surface in advance, the thickness of the photoresist coating will be uneven, resulting in pattern missing and affecting the yield of the semiconductor device.

[0089] The present application provides a method for coating photoresist on a high-step substrate, by which a certain amount of diluent is left on the substrate surface during the spraying of diluent, the dilution efficiency of the photoresist and the fluidity of the photoresist are improved, and the purpose of filling the high-step substrate is achieved through self-leveling of the photoresist, thereby improving the quality of photoresist coating. In addition, the present application also provides an optimal rotation speed range required for self-leveling of the photoresist, which can well solve the problem of uneven coverage of the photoresist layer caused by too low or too high self-leveling speed, and the problem that the photoresist layer is thin in the middle and thick at the edges, thereby helping to improve the yield of semiconductor devices.

[0090] The above describes the basic principles, main features and advantages of the present application. Those skilled in the art should understand that the present application is not limited by the above embodiments, and the above embodiments and the specification only describe the principles of the present application. The present application may have various changes and improvements without departing from the spirit and scope of the present application, and these changes and improvements fall within the scope of the present application for which protection is sought. The scope of protection claimed by the present application is defined by the attached claims and their equivalents.

Claims

1. A photoresist coating method suitable for high-step substrates, It is characterized in that The following steps are involved: S1. Place the substrate to be coated with photoresist on a wafer stage, and the wafer stage maintains a first rotation speed v 1 , v 1 ≥1500 rpm, spray the diluent onto the surface of the substrate for a spraying time of t 1 , so that the surface of the substrate is wetted; S2. Adjust the rotation speed of the wafer carrier to a second rotation speed v 2 , continue to spray the diluent, and the wafer stage continues to rotate for time t 2 The ratio of the volume of the sprayed diluent to the volume of the photoresist sprayed in step S3 is 1:1 to 1:5, v 2 <500 rpm; S3. The wafer stage maintains v 2 The photoresist is sprayed onto the substrate surface in step S2, and after spraying, the wafer stage is kept at a third speed v 3 , making the photoresist self-leveling, v 2 <v 3 ; S4. Adjust the speed of the wafer stage to the process preset speed v 4 , a photoresist layer of preset thickness is obtained on the surface of the substrate.

2. The photoresist coating method according to claim 1, It is characterized in that The ratio of the volume of the diluent sprayed in step S2 to the volume of the photoresist sprayed in step S3 is 1:1 to 1:

3.

3. The photoresist coating method according to claim 2, It is characterized in that The ratio of the volume of the diluent sprayed in step S2 to the volume of the photoresist sprayed in step S3 is 1:

2.

4. The photoresist coating method according to claim 1, It is characterized in that t 2 ≤3s。 5. The photoresist coating method according to claim 4, It is characterized in that v 2 100~200 rpm, t 2 ≤3s.

6. The photoresist coating method according to claim 4, It is characterized in that t 1 ≤5s。 7. The photoresist coating method according to claim 6, It is characterized in that v 1 1500~2500 rpm, t 1 ≤3s.

8. The photoresist coating method according to claim 4, It is characterized in that v 3 700~1000 rpm, t 3 ≤5s.

9. The photoresist coating method according to any one of claims 1 to 8, It is characterized in that In step S3, the viscosity of the sprayed photoresist is not less than 29 cp.

10. The photoresist coating method according to any one of claims 1 to 8, It is characterized in that The diluent is an inactive diluent, and includes one or more combinations of the following: propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate.

Citation Information