Low-temperature silver paste adaptive to flexible substrate mask and preparation method of low-temperature silver paste

The low-temperature silver paste, which combines polymer resins and abrasion-resistant additives, solves the problems of poor abrasion resistance and high-temperature curing in flexible base masks, achieving low-temperature curing and improved abrasion resistance, thus enhancing the stability of the mask during use.

CN119049798APending Publication Date: 2024-11-29运明双
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411260449.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing silver pastes have poor abrasion resistance in flexible substrate films and require high curing temperatures, making them prone to damage and unable to adapt to high-temperature environments during use.

Method used

By combining high-molecular resins, low-temperature curing agents, and wear-resistant additives, and by combining polyurethane resin with polystyrene-poly(ethylene-butene)-polystyrene block copolymer resin, using ester and ether solvents, and adding organosilicon anti-scratch and wear-resistant hand feel agent, a low-temperature silver paste is formed, ensuring that the silver paste cures at low temperature and has wear resistance.

Benefits of technology

This technology enables the silver paste to cure at low temperatures, improving the abrasion resistance and oxidation resistance of flexible substrate masks, reducing the risk of scratches, and enhancing the stability of mask use and the quality of the finished product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of flexible substrate mask silver paste, in particular to low-temperature silver paste adaptive to a flexible substrate mask, which comprises the following components: 5-9 parts of polymer resin, 30-45 parts of organic solvent, 0.5-2 parts of curing agent, 0.5-2 parts of adhesion promoter, 0.5-2 parts of wear-resistant additive and 45-60 parts of conductive silver powder. The polymer resin comprises polyurethane resin and polystyrene-poly (ethylene-butylene)-polystyrene block copolymer resin, and the ratio of the polyurethane resin to the polystyrene-poly (ethylene-butylene)-polystyrene block copolymer resin is (2.5-5): 1. According to the invention, the combination of two polymer resins is used, the polyurethane resin provides mechanical strength and certain flexibility for the silver paste, and the high-elasticity polystyrene-poly (ethylene-butylene)-polystyrene block copolymer resin is introduced, so that the flexibility of a cured silver paste film layer is further improved; and the silver paste conductive circuit is prevented from being bent and damaged in the mask wearing and pasting process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silver paste for flexible substrate masks, and in particular to a low-temperature silver paste suitable for flexible substrate masks and a preparation method thereof. Background Art

[0002] When low-temperature silver paste is mixed, it is bonded with polymer resin as the bonding phase, and is evenly dispersed with organic solvents and additives to form a slurry-like mixture. By heating, drying or curing, the solvent evaporates and the resin cross-links to form a film, thus forming a conductive circuit.

[0003] Existing silver paste electrodes are at risk of bending, folding, abrasion, and scratching during the wearing and application of facial masks, and are also subject to erosion by water, oxygen, sweat, and cosmetics. In addition, during the production process of facial masks, flexible fabric substrates often cannot withstand temperatures above 100°C, so a high curing temperature is required for the low-temperature silver paste. Summary of the invention

[0004] The object of the present invention is to provide a low-temperature silver paste suitable for a flexible substrate mask and a preparation method thereof, so as to solve the problems of poor wear resistance and high temperature requirements of the silver paste mentioned in the background technology.

[0005] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is: a low-temperature silver paste suitable for a flexible substrate mask, comprising the following components: 5 to 9 parts of a polymer resin, 30 to 45 parts of an organic solvent, 0.5 to 2 parts of a curing agent, 0.5 to 2 parts of an adhesion promoter, 0.5 to 2 parts of an anti-wear agent, and 45 to 60 parts of a conductive silver powder; the polymer resin comprises a polyurethane resin and a polystyrene-poly (ethylene-butylene)-polystyrene block copolymer resin, and the ratio of the polyurethane resin to the polystyrene-poly (ethylene-butylene)-polystyrene block copolymer resin is 2.5 to 5:1; The polyurethane resin is a combination of one or more of Lubrizol 5778, 5707, 5712, 5715, 5719, Huntsman 5836P, Covestro 385A, 385E, 385S; the hydrogenated styrene-butadiene block copolymer resin is a combination of one or more of Kraton G1641H, G1645MO, G1650M, G1651H, G1652M, G1654H, MD1646, Kuraray S-8004, S-8006, S-8007, Asahi Kasei H1077, H1285, H1053.

[0006] Preferably, the organic solvent is a combination of one or more ester or ether solvents with a boiling point of 140 to 190° C., and the ester solvent is a combination of one or more of amyl acetate, isoamyl acetate, n-butyl propionate, propylene glycol methyl ether acetate, and ethylene glycol ethyl ether acetate.

[0007] Preferably, the ether solvent is a combination of one or more of ethylene glycol propyl ether, ethylene glycol butyl ether, propylene glycol butyl ether and dipropylene glycol methyl ether.

[0008] Preferably, the curing agent is a blocked isocyanate latent curing agent, the deblocking temperature is not higher than 90° C., and the blocked isocyanate latent curing agent is one of Asahi Kasei MF-K60X, Mitsui XB-G282, and Lanxess Trixene BI 7963.

[0009] Preferably, the adhesion promoter is a silane coupling agent, and the silane coupling agent is a combination of one or more of KH-171, KH-172, KH-550, KH-560, KH-570, and KH-792.

[0010] Preferably, the wear-resistant additive is an organosilicon anti-scratch and wear-resistant feel agent, and the organosilicon anti-scratch and wear-resistant feel agent is one of Dow DC-18, DC-51, DC-57, BYK-333, Silok-51H, Silok-87, and Silok-9180H.

[0011] Preferably, the conductive silver powder includes micron-sized flaky silver powder and micron-sized spherical silver powder, and the ratio of the micron-sized flaky silver powder to the micron-sized spherical silver powder in the conductive silver powder is 3 to 8:1.

[0012] Preferably, the average particle size of the micron-sized silver flake powder is 2.0-5.0 μm, and the tap density is 1.5-3.0 g / cm3; the average particle size of the micron-sized spherical silver powder is 0.8-1.5 μm, and the tap density is 2.5-4.0 g / cm3.

[0013] Preferably, the low-temperature silver paste is suitable for facial masks, neck masks, pleural masks, peritoneal masks, buttocks masks, etc.

[0014] The method for preparing the low-temperature silver paste suitable for the flexible substrate mask of the present invention comprises the following steps: S1, weighing a polymer resin and an organic solvent according to a weight ratio, mixing and stirring at 60-90° C. until they are uniformly dissolved and dispersed, filtering with a 400-mesh filter to remove impurities, and cooling to room temperature for use; S2, weighing an organic carrier, a curing agent, an adhesion promoter and an anti-wear agent according to a weight ratio and uniformly mixing them in a planetary disperser at a speed of 1000 to 1500 rpm; S3, weigh the silver paste matrix and the conductive silver powder according to the weight ratio, mix them evenly in a planetary disperser, and disperse them at a speed of 1000-1500 rpm for 1-2 hours, then put them into a three-roll grinder for grinding. After grinding to a fineness of less than 10 μm, remove the bubbles in a vacuum degassing machine to obtain a low-temperature silver paste suitable for a flexible base mask.

[0015] Beneficial effects of the present invention: 1. The low-temperature silver paste uses a combination of two polymer resins. The polyurethane resin provides mechanical strength and a certain degree of flexibility for the silver paste. The introduction of highly elastic polystyrene-poly (ethylene-butylene)-polystyrene block copolymer resin further improves the flexibility of the silver paste film layer after curing, preventing the silver paste conductive circuit from bending and bending during the mask wearing and application process. At the same time, the polystyrene-poly (ethylene-butylene)-polystyrene block copolymer resin structure does not contain unsaturated double bonds and has stable performance, so that the silver paste has excellent antioxidant, chemical resistance, and aging resistance. 2. The low-temperature silver paste has the characteristics of low-temperature curing at 90°C through the combination of ester and ether solvents, which prevents the silver paste from damaging the mask base due to excessively high curing temperature. At the same time, it avoids the use of ketone solvents that are highly corrosive to the mask base, thereby improving the quality of the finished mask. 3. The low-temperature silver paste is added with silicone anti-scratch and wear-resistant feel agent. After the silver paste is cured, the silicone component migrates to the surface of the silver paste to form a protective layer, making the silver paste film layer smooth and wear-resistant, reducing the damage to the silver paste conductive circuit caused by scratches during the use of the mask, and blocking the intrusion of water, oxygen and chemical components into the silver paste, thereby improving stability. DETAILED DESCRIPTION

[0016] The present invention will be further described below in conjunction with the embodiments. Example 1

[0017] The low-temperature silver paste suitable for the flexible substrate mask described in this embodiment is prepared by the following steps: (1) Preparation of organic carrier: Weigh 45g of polyurethane resin Lubrizol 5715, 15g of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer resin Kraton G1461H, 230g of propylene glycol methyl ether acetate and 120g of ethylene glycol butyl ether, mix and stir at 80°C until uniformly dissolved and dispersed, filter with a 400-mesh filter to remove impurities, and cool to room temperature for use.

[0018] (2) Preparation of silver paste matrix: The organic carrier prepared in step (1), 10 g of curing agent Asahi Kasei MF-K60X, 10 g of adhesion promoter KH-560 and 10 g of wear-resistant additive Dow DC51 were weighed and uniformly mixed in a planetary disperser at a speed of 1200 rpm.

[0019] (3) Production of silver paste: The silver paste matrix prepared in step (2), 430 g of micron-sized flaky silver powder and 130 g of micron-sized spherical silver powder were weighed and mixed evenly in a planetary disperser at a dispersion speed of 1200 rpm for 1.5 h, and then put into a three-roll grinder for grinding. After grinding to a fineness of less than 10 μm, the bubbles were removed in a vacuum degassing machine to obtain the low-temperature silver paste suitable for the flexible substrate mask of the present invention; Example 2

[0020] The low-temperature silver paste suitable for the flexible substrate mask described in this embodiment is prepared by the following steps: (1) Preparation of organic carrier: Weigh 56 g of polyurethane resin Lubrizol 5778, 14 g of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer resin Kraton MD1646, 200 g of propylene glycol methyl ether acetate and 150 g of propylene glycol butyl ether, mix and stir at 80°C until uniformly dissolved and dispersed, filter with a 400-mesh filter to remove impurities, and cool to room temperature for use.

[0021] (2) Preparation of silver paste matrix: The organic vehicle prepared in step (1), 10 g of curing agent Asahi Kasei MF-K60X, 10 g of adhesion promoter KH-560 and 10 g of wear-resistant additive Dow DC51 were weighed and uniformly mixed in a planetary disperser at a speed of 1200 rpm.

[0022] (3) Production of silver paste: Weigh the silver paste base prepared in step (2), 450 g of micron-sized flaky silver powder and 100 g of micron-sized spherical silver powder, mix them evenly in a planetary disperser at a dispersion speed of 1200 rpm for 1.5 h, and then put them into a three-roll grinder for grinding. After grinding to a fineness of less than 10 μm, remove bubbles in a vacuum degassing machine to obtain the low-temperature silver paste suitable for flexible substrate masks as described in the present invention. Example 3

[0023] The low-temperature silver paste suitable for the flexible substrate mask described in this embodiment is prepared by the following steps: (1) Preparation of organic carrier: Weigh 65 g of polyurethane resin Huntsman 5836P, 15 g of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer resin Kuraray S-8006, 250 g of isoamyl acetate and 150 g of dipropylene glycol methyl ether, mix and stir at 80°C until uniformly dissolved and dispersed, filter with a 400-mesh filter to remove impurities, and cool to room temperature for use.

[0024] (2) Preparation of silver paste matrix: The organic carrier prepared in step (1), 10 g curing agent Mitsui XB-G282, 10 g adhesion promoter KH-570 and 10 g wear-resistant additive Silok-51H were weighed and uniformly mixed in a planetary disperser at a speed of 1200 rpm.

[0025] (3) Production of silver paste: Weigh the silver paste base prepared in step (2), 430 g of micron-sized flaky silver powder and 60 g of micron-sized spherical silver powder, mix them evenly in a planetary disperser at a dispersion speed of 1200 rpm for 1.5 h, and then put them into a three-roll grinder for grinding. After grinding to a fineness of less than 10 μm, remove bubbles in a vacuum degassing machine to obtain the low-temperature silver paste suitable for flexible substrate masks described in the present invention.

[0026] The method is basically the same as Example 1, except that the amount of polyurethane resin Lubrizol 5715 added is 36 g, and the amount of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer resin Kraton G1461H added is 24 g, that is, the total weight of the two remains unchanged, and the weight ratio becomes 1.5:1. The method is basically the same as Example 1, except that the amount of polyurethane resin Lubrizol 5715 added is 52.5 g, and the amount of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer resin Kraton G1461H added is 7.5 g, that is, the total weight of the two remains unchanged and the weight ratio becomes 7:1. The method is basically the same as Example 1, except that the wear-resistant additive Dow DC51 is not added.

[0027] Performance Test: The low-temperature silver paste prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 was printed on a non-woven fabric substrate by gravure printing. The curing conditions were 90°C for 30 min. The length of the silver paste line was 100 mm, the width was 1 mm, and the dry film thickness was 9 to 12 μm. The square resistance was calculated based on the resistance, length, width and dry film thickness of the silver paste line. The hardness was tested using a pencil hardness tester and the adhesion was tested using the hundred-grid method. In the bending resistance experiment, the cured silver paste strips were folded forward and backward, and the number of bends when the resistance increased by 100% was recorded (1 bending forward and backward was recorded as 1 time). In terms of weather resistance testing, the resistance change of the silver paste strips before and after constant temperature and humidity (85°C, 85%RH, 240h) and salt spray test (5%NaCl solution, 35°C, 96h) was judged.

[0028] The test results are shown in the following table: project Square resistance mΩ / þ / mil hardness Adhesion Bending times Constant temperature and humidity resistance change% Salt spray resistance change% Example 1 20.4 2H 4B 29 +6.5 +7.4 Example 2 17.5 2H 4B 24 +7.2 +8.7 Example 3 25.8 2H 4B 26 +5.4 +5.9 Comparative Example 1 22.1 H 4B 13 +6.7 +7.5 Comparative Example 2 18.7 2H 4B 9 +10.2 +13.0 Comparative Example 3 19.9 H 4B 18 +13.6 +17.2 From the above test results, it can be seen that the low-temperature silver paste prepared by the present invention, through the polymer resin system, functional additives and component ratio design, Examples 1 to 3 all show good conductivity, excellent bending resistance and weather resistance. In summary, the low-temperature silver paste of the present invention has excellent adaptability to the application of flexible substrate masks.

[0029] The embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of those skilled in the art without departing from the spirit of the present invention.

Claims

1. A low-temperature silver paste suitable for flexible substrate masks, Features: The invention comprises the following components: 5 to 9 parts of polymer resin, 30 to 45 parts of organic solvent, 0.5 to 2 parts of curing agent, 0.5 to 2 parts of adhesion promoter, 0.5 to 2 parts of wear-resistant additive, and 45 to 60 parts of conductive silver powder; The polymer resin includes polyurethane resin and polystyrene-poly (ethylene-butylene)-polystyrene block copolymer resin, and the ratio of polyurethane resin to polystyrene-poly (ethylene-butylene)-polystyrene block copolymer resin is 2.5-5:1; The polyurethane resin is a combination of one or more of Lubrizol 5778, 5707, 5712, 5715, 5719, Huntsman 5836P, Covestro 385A, 385E, 385S; The hydrogenated styrene-butadiene block copolymer resin is a combination of one or more of Kraton G1641H, G1645MO, G1650M, G1651H, G1652M, G1654H, MD1646, Kuraray S-8004, S-8006, S-8007, Asahi Kasei H1077, H1285, and H1053.

2. The low-temperature silver paste for adapting to a flexible substrate mask according to claim 1, Features: The organic solvent is a combination of one or more ester or ether solvents with a boiling point of 140 to 190° C., and the ester solvent is a combination of one or more of amyl acetate, isoamyl acetate, n-butyl propionate, propylene glycol methyl ether acetate, and ethylene glycol ethyl ether acetate.

3. The low-temperature silver paste for adapting to a flexible substrate mask according to claim 1, Features: The ether solvent is a combination of one or more of ethylene glycol propyl ether, ethylene glycol butyl ether, propylene glycol butyl ether and dipropylene glycol methyl ether.

4. The low-temperature silver paste for adapting to a flexible substrate mask according to claim 1, Features: The curing agent is a blocked isocyanate latent curing agent, the deblocking temperature is not higher than 90°C, and the blocked isocyanate latent curing agent is one of Asahi Kasei MF-K60X, Mitsui XB-G282, and Lanxess Trixene BI 7963.

5. The low-temperature silver paste for adapting to a flexible substrate mask according to claim 1, Features: The adhesion promoter is a silane coupling agent, and the silane coupling agent is a combination of one or more of KH-171, KH-172, KH-550, KH-560, KH-570, and KH-792.

6. The low-temperature silver paste for adapting to a flexible substrate mask according to claim 1, Features: The wear-resistant additive is an organosilicon anti-scratch and wear-resistant feel agent, and the organosilicon anti-scratch and wear-resistant feel agent is one of Dow DC-18, DC-51, DC-57, BYK-333, Silok-51H, Silok-87, and Silok-9180H.

7. The low-temperature silver paste for adapting to a flexible substrate mask according to claim 1, Features: The conductive silver powder includes micron-sized flaky silver powder and micron-sized spherical silver powder. The ratio of the micron-sized flaky silver powder to the micron-sized spherical silver powder in the conductive silver powder is 3 to 8:

1.

8. The low-temperature silver paste for adapting to a flexible substrate mask according to claim 1, Features: The average particle size of micron-sized flake silver powder is 2.0-5.0μm, and the tap density is 1.5-3.0g / cm3. The average particle size of micron-sized spherical silver powder is 0.8-1.5μm, and the tap density is 2.5-4.0g / cm3.

9. The low-temperature silver paste for adapting to a flexible substrate mask according to claim 1, Features: This low-temperature silver paste is suitable for facial masks, neck masks, pleural masks, peritoneal masks, buttocks masks, etc.

10. The method for preparing low-temperature silver suitable for a flexible substrate mask according to any one of claims 1 to 9, Features: The steps include: S1, weighing a polymer resin and an organic solvent according to a weight ratio, mixing and stirring at 60-90° C. until they are uniformly dissolved and dispersed, filtering with a 400-mesh filter to remove impurities, and cooling to room temperature for use; S2, weighing an organic carrier, a curing agent, an adhesion promoter and an anti-wear agent according to a weight ratio and uniformly mixing them in a planetary disperser at a speed of 1000 to 1500 rpm; S3, weigh the silver paste matrix and the conductive silver powder according to the weight ratio, mix them evenly in a planetary disperser, and disperse them at a speed of 1000-1500 rpm for 1-2 hours, then put them into a three-roll grinder for grinding. After grinding to a fineness of less than 10 μm, remove the bubbles in a vacuum degassing machine to obtain a low-temperature silver paste suitable for a flexible base mask.