Silicon carbide-based integrated SBD and SGT device and preparation method thereof

By adding polysilicon layer and metal link holes at the bottom of the trench in the silicon carbide-based integrated SBD and SGT devices, the problem of easy breakdown of the bottom gate oxide layer of the silicon carbide trench MOSFET device is solved, and the reliability and performance of the device are improved .

CN119049972APending Publication Date: 2024-11-29SHENZHEN BASIC SEMICON LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411001566.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

When the silicon carbide trench MOSFET device is not used in anti-parallel with the diode, it is impossible to avoid the problem of easy breakdown at the bottom of the trench caused by excessive electric field of the bottom gate oxide layer, which limits its promotion in practical applications.

Method used

During the preparation of silicon carbide-based integrated SBD and SGT devices, a polysilicon layer is deposited at the bottom of the trench and a metal link hole is formed on the polysilicon layer, increasing the thickness of the gate oxide layer and achieving the link between the source and the shield gate. This reduces the gate capacitance.

Benefits of technology

It effectively overcomes the problem of easy breakdown of the gate oxide layer at the bottom of the MOSFET device, improves the reliability and performance of the device, and avoids performance degradation caused by the increase in gate capacitance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049972A_ABST
    Figure CN119049972A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon carbide-based integrated SBD and SGT device and a preparation method thereof, and the method comprises the steps: obtaining an N-type silicon carbide substrate, growing an N-type silicon carbide epitaxial layer on the front surface of the N-type silicon carbide substrate, and generating a drain metal layer on the back surface of the N-type silicon carbide substrate; sequentially injecting P-type impurities and N-type impurities into a first region on the top surface of the N-type silicon carbide epitaxial layer to form an N-type doped region and a first P-type doped region which are adjacent to each other; performing etching in the first region through a photoetching process to form a groove; sequentially generating a first gate oxide layer, a polycrystalline silicon layer and a shield gate from outside to inside in the trench; forming a metal link hole in the polycrystalline silicon layer; depositing a second gate oxide layer at the opening of the groove to cover the opening of the groove; and growing a source metal layer on the top surface of the second gate oxide layer. By using the method disclosed by the invention, the problem that the gate oxide layers at the two corners of the bottom of the groove of the silicon carbide groove type MOSFET device are easy to break down in the prior art can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chips and relates to a silicon carbide-based integrated SBD and SGT device and a preparation method thereof. Background Art

[0002] Silicon carbide (SiC), as a typical representative of the third generation of semiconductors, not only has a wide bandgap, but also has advantages such as high breakdown voltage, high thermal conductivity, and high electron saturation rate. Therefore, power electronic devices made of silicon carbide materials have higher withstand voltage, greater current carrying capacity, and higher operating frequency, and can work in high-frequency and high-temperature environments with high reliability, and can be suitable for harsh working environments. Therefore, silicon carbide materials, as third-generation power electronic devices, have become the most important development direction of power electronic technology, and have important application prospects in military and civil fields.

[0003] Silicon carbide metal-oxide-semiconductor field-effect transistor (MOSFET) devices are next-generation semiconductor devices made of wide-bandgap semiconductor material silicon carbide. With its excellent material properties, it is considered to be a new generation of semiconductor power devices with the potential to replace traditional silicon-based superjunction MOSFET and insulated gate bipolar transistor (IGBT) devices in full-power applications. However, due to the unsatisfactory channel of planar silicon carbide MOSFET, the MOSFET channel mobility is too low, which greatly limits the on-state current density of silicon carbide MOSFET. Therefore, silicon carbide trench MOSFETs with higher channel density and thus greater on-state current density have received extensive attention and research. Although silicon carbide trench MOSFETs have lower on-state resistance and more compact cell layout, the problem of excessively high electric field in the bottom gate oxide layer brings reliability problems to the long-term use of silicon carbide trench MOSFETs.

[0004] In order to overcome the problem of too high electric field in the bottom gate oxide layer of silicon carbide trench MOSFET, silicon carbide MOSFET devices usually need to be used in anti-parallel with a diode in applications. There are usually two ways to achieve this goal. One is to directly use the parasitic P / N-diode formed by the P-type base region of the device and the silicon carbide N-drift region, but the parasitic silicon carbide diode has a large on-state voltage drop and poor reverse recovery characteristics, resulting in high power loss, which is not conducive to its promotion in the power market. At the same time, the low working speed leads to low working efficiency, which is extremely unfavorable for silicon carbide MOSFET devices in actual circuit applications; the second is to use the device in anti-parallel with an external diode through packaging, but this method increases the number of metal wire interconnections and increases parasitic inductance, which is not conducive to improving system reliability; at the same time, due to the increase in the number of devices, the system volume increases, the supporting heat dissipation requirements also increase, and the packaging cost also increases. The above problems have hindered the promotion of silicon carbide MOSFET devices in many practical applications.

[0005] In summary, there is an urgent need in the art for a silicon carbide trench MOSFET device that can avoid the problem of gate oxide layers at two corners of the bottom of the trench being easily broken down due to excessive electric field in the gate oxide layer at the bottom of the MOSFET device when not used in anti-parallel with a diode. Summary of the invention

[0006] The present invention provides a silicon carbide-based integrated SBD and SGT device and a preparation method thereof, which are used to solve the problem in the prior art that when a silicon carbide trench MOSFET device is not used in anti-parallel with a diode, the gate oxide layer at the two corners of the bottom of the trench cannot be easily broken down due to the excessively high electric field of the gate oxide layer at the bottom of the MOSFET device.

[0007] In order to solve the above technical problems, in a first aspect, the present invention provides a method for preparing a silicon carbide-based integrated SBD and SGT device, comprising:

[0008] Obtaining an N-type silicon carbide substrate, growing an N-type silicon carbide epitaxial layer on the front surface of the N-type silicon carbide substrate, and generating a drain metal layer on the back surface of the N-type silicon carbide substrate;

[0009] Sequentially implanting P-type impurities and N-type impurities into a first region of the top surface of the N-type silicon carbide epitaxial layer to form adjacent N-type doped regions and a first P-type doped region;

[0010] Etching a groove in the first region by a photolithography process, wherein the groove passes through the N-type doped region and the first P-type doped region;

[0011] In the trench, a first gate oxide layer, a polysilicon layer and a shielding gate are sequentially generated from outside to inside, wherein the polysilicon layer is located in the first gate oxide layer;

[0012] forming a metal link hole on the polysilicon layer;

[0013] Depositing a second gate oxide layer at the opening of the trench to cover the trench opening;

[0014] A source metal layer is grown on the top surface of the second gate oxide layer, wherein the source metal layer is connected to the metal link hole.

[0015] Optionally, the step of sequentially generating a first gate oxide layer, a polysilicon layer and a shielding gate from outside to inside in the trench includes:

[0016] A third gate oxide layer is deposited on the bottom and sidewalls of the trench by using a SAUSG method and a SACVD process;

[0017] Depositing a polysilicon layer on the outer surface of the third gate oxide layer;

[0018] Etching back the polysilicon layer until the thickness of the polysilicon layer is within a preset range;

[0019] generating a fourth gate oxide layer at the outermost layer of the trench;

[0020] In the trench, a D poly layer is deposited on an outer surface of the fourth gate oxide layer to form a shielding gate.

[0021] Optionally, generating a fourth gate oxide layer at the outermost layer of the current trench comprises:

[0022] Etching the third gate oxide layer until the third gate oxide layer is flush with the polysilicon layer;

[0023] A fourth gate oxide layer is grown on an outer surface of the trench, an outer surface of the third gate oxide layer, and an outer surface of the polysilicon layer.

[0024] Optionally, after sequentially implanting P-type impurities and N-type impurities into a first region in the top surface of the N-type silicon carbide epitaxial layer, and before etching to form a trench in the first region by a photolithography process, the method further includes:

[0025] P-type impurities are implanted into a second region of the top surface to form a second P-type doped region, wherein the second P-type doped region is adjacent to both the N-type doped region and the first P-type doped region.

[0026] Optionally, after depositing the second gate oxide layer at the opening of the trench and before growing the source metal layer on the top surface of the second gate oxide layer, the method further includes:

[0027] An ohmic metal layer and a Schottky barrier diode (SBD) layer are respectively generated in a second region and a third region of the N-type silicon carbide epitaxial layer, wherein the third region is adjacent to the second region.

[0028] Optionally, the step of respectively generating an ohmic metal layer and a Schottky barrier diode SBD layer in the second region and the third region of the N-type silicon carbide epitaxial layer comprises:

[0029] depositing an oxide insulating layer on a third region of the N-type silicon carbide epitaxial layer;

[0030] Depositing an ohmic metal layer on the top surface of the N-type silicon carbide epitaxial layer to form an alloy layer of the ohmic metal layer and silicon carbide;

[0031] removing the alloy layer on the surface of the oxide insulating layer and the second gate oxide layer;

[0032] Etching the oxidized insulating layer and removing the photoresist by a photolithography process to form an SBD generation area;

[0033] sputtering a Schottky metal in the SBD generation region and etching the Schottky metal through a photolithography process;

[0034] The etched Schottky metal is alloyed with silicon carbide to form a SBD layer.

[0035] Optionally, the thickness of the first gate oxide layer is 2000-3000 Å.

[0036] Optionally, the thickness of the polysilicon layer is 5000-6000A.

[0037] Optionally, the second gate oxide layer has a thickness of 500-600 Å.

[0038] In a second aspect, the present invention provides a silicon carbide-based integrated SBD and SGT device, comprising:

[0039] N-type silicon carbide substrate;

[0040] A drain metal layer is sputtered on the back side of the N-type silicon carbide substrate;

[0041] An N-type silicon carbide epitaxial layer grown on the front surface of the N-type silicon carbide substrate;

[0042] A first P-type doped region, located inside the N-type silicon carbide epitaxial layer;

[0043] an N-type doped region located inside the N-type silicon carbide epitaxial layer and between a top surface of the N-type silicon carbide epitaxial layer and the first P-type doped region;

[0044] A second P-type doped region, located inside the N-type silicon carbide epitaxial layer, adjacent to both the N-type doped region and the first P-type doped region;

[0045] A groove is etched in a first region of the top surface of the N-type silicon carbide epitaxial layer and penetrates the first P-type doped region and the N-type doped region;

[0046] a first gate oxide layer deposited on an outer surface of the trench;

[0047] A polysilicon layer, located in the first gate oxide layer, and having a metal link hole on the polysilicon layer;

[0048] A shielding gate, deposited on an outer surface of the first gate oxide layer;

[0049] A second gate oxide layer is deposited at the opening of the trench and covers the opening;

[0050] an ohmic metal layer, adjacent to the second gate oxide layer and located in a second region of the top surface of the N-type silicon carbide epitaxial layer, the second region being opposite to the second P-type doped region;

[0051] an SBD metal layer, adjacent to the ohmic metal layer and formed in a third region of the top surface of the N-type silicon carbide epitaxial layer;

[0052] The source metal layer covers the SBD metal layer, the ohmic metal layer and the second gate oxide layer.

[0053] Compared with the prior art, the method for preparing a silicon carbide-based SBD and SGT device provided by the present invention has the following beneficial effects:

[0054] In the process of preparing silicon carbide-based integrated SBD and SGT devices, a polysilicon layer is generated in the first gate oxide layer deposited at the bottom of the trench, so that the actual thickness of the first gate oxide layer deposited at the bottom of the trench is the sum of the thickness of the gate oxide layer in the first gate oxide layer and the thickness of the polysilicon layer. It can be understood that compared with the prior art that there is only a gate oxide layer at the bottom of the trench, the thickness of the gate oxide layer at the bottom of the trench of the silicon carbide-based integrated SBD and SGT devices prepared by the present invention can be greatly increased compared with the thickness of the gate oxide layer in the prior art, thereby overcoming the problem that the gate oxide layer at the two corners of the bottom of the trench is easily broken down due to the excessively high electric field of the gate oxide layer at the bottom of the MOSFET device in the prior art; in addition, when the thickness of the gate oxide layer in the trench of the trench MOSFET device increases, the gate capacitance increases, while in the present invention, a polysilicon layer is generated in the first gate oxide layer, and a metal link hole is formed on the polysilicon layer, and the source metal layer is linked to the polysilicon layer through the metal link hole to achieve the link between the source and the shielding gate, thereby reducing the gate capacitance. In summary, the present invention can solve the problem in the prior art that when a silicon carbide trench MOSFET device is not used in anti-parallel with a diode, the gate oxide layer at the two corners of the bottom of the trench cannot be easily broken down due to the excessively high electric field of the gate oxide layer at the bottom of the MOSFET device. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only part of the embodiments of the present invention, rather than all of the embodiments. For ordinary technicians in this field, without paying creative work, other drawings obtained based on these drawings all fall within the scope of protection of this application.

[0056] Figure 1 It is a flow chart of a method for preparing a silicon carbide-based SBD and SGT device provided in an embodiment of the present invention;

[0057] Figures 2 to 20 It is a structural schematic diagram corresponding to the preparation process of the silicon carbide-based SBD and SGT devices provided in an embodiment of the present invention;

[0058] Fig.21 It is a schematic structural diagram of a silicon carbide-based SBD and SGT device provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0059] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0060] In order to make the description of the disclosed content more detailed and complete, the following is an illustrative description of the implementation mode and specific examples of the present invention; however, this is not the only form of implementing or applying the specific embodiments of the present invention. The implementation mode covers the features of multiple specific embodiments and the method steps and their sequence for constructing and operating these specific embodiments. However, other specific embodiments can also be used to achieve the same or equal functions and step sequences. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0061] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the numbers used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein.

[0062] In addition, in the description of the embodiments of the present application, "multiple" refers to two or more than two, and other quantifiers are similar and should be understood. The preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention. In addition, the embodiments of the present application and the features therein may be combined with each other if there is no conflict.

[0063] like Figure 1 The flowchart shown is a method for preparing a silicon carbide-based integrated SBD and shielded gate transistor (SGT) device provided by an embodiment of the present invention, which includes the following steps.

[0064] Step S101 : obtaining an N-type silicon carbide substrate 100 , growing an N-type silicon carbide epitaxial layer 200 on the front surface of the N-type silicon carbide substrate 100 , and generating a drain metal layer 300 on the back surface of the N-type silicon carbide substrate 100 .

[0065] Specifically, the specific structure formed in this step is as follows Figure 2 shown.

[0066] It should be noted that the N-type silicon carbide substrate 100 refers to a silicon carbide material that is doped with N-type impurity atoms (such as nitrogen or phosphorus) to become an N-type semiconductor.

[0067] The N-type silicon carbide epitaxial layer 200 is a layer of N-type semiconductor material deposited on the N-type silicon carbide substrate 100 by epitaxial growth technology, wherein a gas containing a nitrogen source reacts with a gas containing a carbon source and a silicon source at a high temperature and is deposited on the substrate to form an epitaxial layer. N-type dopants (such as nitrogen or phosphorus) are introduced during the growth process to ensure that the material has sufficient free electrons, thereby exhibiting the electrical characteristics of an N-type semiconductor.

[0068] Optionally, the thickness of the N-type silicon carbide substrate 100 may be 300-400 um (micrometers), because if the thickness of the substrate is too thin, it is easy to break during the preparation process, and if the thickness of the substrate is too thick, it will cause waste. The doping concentration of the substrate may be greater than 1e19 / cm 3 (cubic centimeters) to ensure sufficiently low resistance.

[0069] It should be noted that the doping concentration of the N-type silicon carbide epitaxial layer 200 must be lower than the doping concentration of the N-type silicon carbide substrate 100 because the substrate is used for conducting and does not withstand voltage. Therefore, the epitaxial layer needs to have a lower doping concentration to withstand voltage.

[0070] It should be noted that the front side of the N-type silicon carbide substrate 100 is the C-side of the silicon carbide crystal. The lattice on the C-side has a high degree of lattice matching with the substrate, which is beneficial to the growth quality and lattice matching of the epitaxial layer and reduces the defect density. In addition, the surface energy of the C-side is low, making the epitaxial layer grow more stably thereon. Therefore, choosing to perform silicon carbide epitaxy on the C-side can obtain a higher quality epitaxial layer and minimize the defects caused by lattice mismatch.

[0071] Optionally, the doping concentration of the N-type silicon carbide epitaxial layer 200 may be 1e15-1e16 / cm 3 , the thickness can be between 10-12um.

[0072] It should be noted that the method of generating the drain metal layer 300 on the back side of the N-type silicon carbide substrate 100 may be any achievable method;

[0073] As a specific example, in the process of generating the drain metal layer 300 on the back side of the N-type silicon carbide substrate 100, a blue film may be firstly attached to the front side of the N-type silicon carbide substrate 100, so that in the subsequent process of thinning the N-type silicon carbide substrate 100, the front side of the N-type silicon carbide substrate 100 is not affected by the subsequent thinning process. The N-type silicon carbide substrate 100 may be further thinned to reduce the overall thickness of the device, thereby reducing parasitic inductance and thermal resistance, and improving heat dissipation efficiency. After the thinning operation is completed, the N-type A blue film protective layer is formed on the front side of the silicon carbide substrate 100 to facilitate subsequent processing and packaging. After removing the blue film, the impurities and residues remaining on the device surface can be cleaned to ensure the quality of the subsequent metallization process. Titanium can be further evaporated on the back side of the N-type silicon carbide substrate 100 to initially form an ohmic contact. Titanium can help subsequent metal layers to better adhere to the silicon carbide substrate. Through laser annealing, titanium, nickel and silver are deposited on the back side of the N-type silicon carbide substrate 100 in sequence, wherein titanium is an adhesion layer, nickel is a barrier layer, and silver is a conductive layer.

[0074] Step S102 , sequentially implanting P-type impurities and N-type impurities into a first region of the top surface of the N-type silicon carbide epitaxial layer 200 to form adjacent N-type doped regions 310 and first P-type doped regions 320 .

[0075] The specific structure formed in this step is as follows Figure 3 and Figure 4 As shown, Figure 3 To form a structural diagram of the first P-type doping region 320, Figure 4 FIG. 3 is a structural diagram for forming an N-type doping region 310 .

[0076] Optionally, the P-type impurities injected in this step may be aluminum, and the N-type impurities injected may be nitrogen.

[0077] Optionally, in the process of injecting P-type impurities in this step, the injection may be performed multiple times with different concentrations to form a first P-type doping region 320 with a concentration gradient. The first P-type doping region 320 is called Pbody. As a specific example, the number of injections of P-type impurities may be 3 to 5 times, and the energy of the first injection of P-type impurities is 30-40kev (kiloelectron volts) and the dose is 1-5e15 / cm 3 The energy of the second injection of P-type impurities is 80-120keV, and the dose is 1-5e13 / cm 3 The third injection energy is 200-300kev and the dose is 15e13 / cm 3 The fourth injection energy is 300-400kev and the dose is 1-5e14 / cm 3 The fifth implantation energy is 400-500kev and the dose is 1-5e15 / cm3 , and the injection temperature of P-type impurities can be as high as 500-600°C (degrees Celsius).

[0078] Optionally, in the process of injecting N-type impurities in this step, the implantation may be performed multiple times with different concentrations to form an N-type doped region 310 with a concentration gradient. As a specific example, the number of N-type impurities implanted may be 3-5 times, the energy of the first N-type impurity implantation may be 20-30kev, and the dose may be 1-5e14 / cm 3 The energy of the second N-type impurity injection can be 30-40keV, and the dose can be 1-5e14 / cm 3 The energy of the third N-type impurity injection can be 50-60kev, and the dose can be 1-5e14 / cm 3 The energy of the fourth N-type impurity injection can be 100-200kev, and the dose can be 1-8e13 / cm 3 , the final junction depth can be 0.2um, and the doping concentration is greater than 1e19 / cm 3 The N-type doped region 310 is formed, and the temperature of the N-type impurities implanted can be at a high temperature of 500-600°C.

[0079] Specifically, before the P-type impurities and the N-type impurities are implanted, an implantation region may be formed by etching on the top surface of the epitaxial layer through a photolithography process. As a specific example, after the epitaxial layer is cleaned, a sandwich structure hard mask 311 (hard mask, HM) is grown on the top surface of the epitaxial layer, wherein the first layer of the HM may be a thermal oxide layer pad ox, and the thickness may be 400-500A. This thermal oxide layer may be used as a shielding layer when P-type impurities are injected, and the thickness uniformity of the thermal oxide layer is better controlled. The second layer may be a polysilicon layer, and this layer may be used as a transition layer, and this layer may be used to connect the first layer and the third layer, so that the endpoint detection signal is strong during etching. The third layer may be low pressure tetraethoxysilane (Low Pressure TetraEthyl OrthoSilicate, LPTEOS), and the thickness may be 2-2.5um. It may be further subjected to high temperature densification, and then photolithography patterning may be performed, and operations of coating, exposure and development may be performed. The thickness of the photoresist may be 2-2.5um, and then etching may be started. Etching may be performed using an inductively coupled plasma (ICP) or transverse capacitively coupled plasma (ICP) with better anisotropy. Plasma, TCP) plasma dry etching, first etch the top LPTEOS, grab the end point to stop at the polysilicon layer, then etch the polysilicon layer, grab the end point to stop at pad ox, then remove the glue and clean it to form the injection area, the final structure is as follows Figure 3 and Figure 4 shown.

[0080] Step S103 , etching to form a trench 400 in the first region by a photolithography process.

[0081] The specific structure formed in this step is as follows Figure 5 shown.

[0082] The trench passes through the N-type doping region 310 and the first P-type doping region 320 .

[0083] In this step, the method of etching to form the groove 400 by a photolithography process may be any feasible method.

[0084] It should be noted that in this step, the trench 400 passes through the N-type doping region 310 and the first P-type doping region 320 , which means that the depth of the trench 400 is greater than or equal to the total depth of the N-type doping region 310 and the first P-type doping region 320 .

[0085] As a specific example, in this step, a hard mask 410 can be generated. Specifically, a 2-2.5um thick plasma enhanced tetraethylorthosilicate (PETEOS) can be grown by a plasma enhanced chemical vapor deposition (PECVD) process, or a corresponding thickness of polyethylene oxide can be grown as a hard mask for silicon carbide trench etching, and then a low pressure chemical vapor deposition (LPCVD) process can be used. Deposition, LPCVD) grows 100-200nm polysilicon (polysilicon can also be replaced by qualified photoresist), the polysilicon can be used as a mask for etching PETEOS, and then a layer of photoresist is coated to serve as a mask for etching polysilicon, and then the photoresist is exposed by a photolithography process, and then the polysilicon is etched, and the photoresist is removed after etching, and then the PETEOS is etched by dry etching (dry etching can ensure that the vertical side wall is etched), the PETEOS angle needs to be vertical greater than 88°, and finally, the silicon carbide groove is etched by an inductively coupled plasma etching (ICP) process under oxygen-rich conditions (the ICP process can provide a higher density plasma), and the groove width and depth of the final etched groove can be 1-1.5um, 2-2.5um, the side wall angle is greater than 88°, the bottom is round (referring to the bottom of the groove has a certain curvature), and the root mean square roughness (RMS) can be less than 0.2nm.

[0086] Before this step, high temperature activation can be used (for example, activation can be performed at a temperature of 1600-1750 degrees Celsius for 20-30 minutes), but high temperature reaction will cause the surface to be rough, making it impossible to process in the later process. For this reason, a layer of carbon film 420 can be sputtered before high temperature activation, and the carbon film 420 can be removed by sulfuric acid corrosion and other processes after high temperature activation. The specific structure is as follows Figure 6 shown.

[0087] Step S104 , forming a first gate oxide layer 430 , a polysilicon layer 440 and a shield gate 450 in sequence from outside to inside in the trench 400 .

[0088] The specific structure in this step is as follows Figure 7 shown.

[0089] The polysilicon layer 440 is located in the first gate oxide layer 430 .

[0090] It should be noted that the method of generating the first gate oxide layer 430 , the polysilicon layer 440 and the shield gate 450 in the trench 400 may be any feasible method, which is not limited in detail herein.

[0091] Step S105 , forming a metal link hole on the polysilicon layer 440 .

[0092] It should be noted that the metal link hole formed on the polysilicon layer 440 can be obtained by etching.

[0093] Step S106 , depositing a second gate oxide layer 460 at the opening of the trench 400 to cover the opening of the trench 400 .

[0094] The specific structure in this step is as follows Figure 8 shown.

[0095] Optionally, the second gate oxide layer 460 in this step may be silicon dioxide. As a specific example, the thickness of the second gate oxide layer 460 deposited at the opening of the trench may be 0.5-1 um.

[0096] Step S107 , growing a source metal layer 461 on the top surface of the second gate oxide layer 460 .

[0097] The specific structure in this step is as follows Fig. 9 shown.

[0098] Wherein, the source metal layer 461 is connected to the metal link hole.

[0099] It should be noted that the source metal layer 461 grown on the top surface of the second gate oxide layer 460 in this step may be grown in any achievable manner.

[0100] It should be noted that the source metal layer 461 in this step can be any metal that can serve as a source metal. For example, the source metal layer 461 in this step can be obtained by growing a certain thickness of aluminum. As a specific example, the thickness of the source metal layer can be 3um-4um.

[0101] After this step, the device can be passivated to form a passivation layer 500. As a specific example, in the process of passivating the device, PETEOS with a thickness of 6000-8000A can be first deposited on the surface of the device, and then 300-500A of plasma enhanced silicon nitride (PESIN) can be further deposited, and finally 6-10um polyimide can be deposited. PETEOS, PESIN and polyimide are deposited on the surface of the device, so that they can play the role of insulation and passivation together, protect the device from damage by external factors, and optimize the electrical performance of the device. The specific structure formed is as follows: Fig.10 shown.

[0102] In this way, in the process of preparing the silicon carbide-based integrated SBD and SGT devices in the embodiment of the present invention, a polysilicon layer 440 is generated in the first gate oxide layer 430 deposited at the bottom of the trench 400, so that the actual thickness of the first gate oxide layer 430 deposited at the bottom of the trench 400 is the sum of the thickness of the gate oxide layer in the first gate oxide layer 430 and the thickness of the polysilicon layer 440. It can be understood that in this way, compared with the prior art in which there is only a gate oxide layer at the bottom of the trench 400, the thickness of the gate oxide layer at the bottom of the trench 400 of the silicon carbide-based integrated SBD and SGT devices prepared in the embodiment of the present invention is greater than that of the prior art in which there is only a gate oxide layer at the bottom of the trench 400. The thickness of the oxide layer can be greatly increased, thereby overcoming the problem in the prior art that the gate oxide layer at the two corners of the bottom of the trench is easily broken down due to the excessively high electric field of the gate oxide layer at the bottom of the MOSFET device; in addition, when the thickness of the gate oxide layer in the trench 400 of the trench MOSFET device increases, the gate capacitance increases, and in the embodiment of the present invention, a polysilicon layer 440 is generated in the first gate oxide layer 430, and a metal link hole is formed on the polysilicon layer 440, and the source metal layer 461 is linked to the polysilicon layer 440 through the metal link hole to achieve the connection between the source and the shielding gate, thereby reducing the gate capacitance. In summary, the embodiment of the present invention can solve the problem in the prior art that the gate oxide layer at the two corners of the bottom of the trench cannot be easily broken down due to the excessively high electric field of the gate oxide layer at the bottom of the MOSFET device when the silicon carbide trench MOSFET device is not used in anti-parallel with a diode.

[0103] In an optional implementation, the first gate oxide layer 430, the polysilicon layer 440 and the shield gate 450 are sequentially generated from outside to inside in the trench 400, including:

[0104] The third gate oxide layer 431 is deposited on the bottom and sidewalls of the trench by using the SAUSG method and the SACVD process. Fig.11 As shown;

[0105] A polysilicon layer 440 is deposited on the outer surface of the third gate oxide layer 431. Fig.12 As shown;

[0106] The polysilicon layer 440 is etched back until the thickness of the polysilicon layer 440 is within a preset range. Fig.13 As shown;

[0107] A fourth gate oxide layer 432 is formed on the outermost layer of the trench. Fig.14 As shown;

[0108] In the trench, a D poly layer is deposited on the outer surface of the fourth gate oxide layer 432 to form a shield gate 450 .

[0109] The stress-targeted uniform sacrificial oxide gapfill (SAUSG) method is adopted. This process can reduce or control the stress generated during the integrated circuit manufacturing process. SAUSG can temporarily relieve structural stress by filling the groove with a material (sacrificial oxide) that can be removed by subsequent processes. SAUSG can eventually form a uniform stress distribution on the groove surface, which helps to improve the performance and reliability of the device; Selective Atmospheric Chemical Vapor Deposition (SACVD) is a technology that can selectively deposit thin films in specified areas without forming deposits in areas where deposition is not required. This technology is very useful for precise material deposition in complex three-dimensional structures. In this process, SACVD is used to deposit the third gate oxide layer 431 at the bottom and side walls of the trench. Compared with the traditional chemical vapor deposition (CVD) process, which can only form a uniform thin film on the entire wafer surface but is difficult to obtain uniform coverage inside structures such as trenches, the third gate oxide layer 431 (i.e., SAUSG) is deposited at the bottom and side walls of the trench 400 by SACVD, which can ensure good electrical isolation and performance control even in three-dimensional structures.

[0110] As a specific example, the thickness of the SAUSG material deposited in the trench may be 2000-3000 Å.

[0111] It should be noted that in order to facilitate the subsequent etching back process, when the polysilicon layer 440 is deposited on the outer surface of the third gate oxide layer 431, the thickness of the polysilicon layer 440 can be made to exceed the opening of the groove 400. As a specific example, the distance that the polysilicon layer 440 exceeds the opening of the groove 400 can be 1-1.5um.

[0112] As a specific example, the polysilicon layer 440 may be etched back by isotropic dry etching until the thickness of the polysilicon layer 440 is within a preset range, for example, the preset range may be 5000-6000 Å.

[0113] As a specific example, when the fourth gate oxide layer 432 is generated in the outermost layer of the groove, the current outer surface of the device can be surface treated with nitric oxide first, and then thermally oxidized in oxygen to grow an oxide layer of a certain thickness (for example, 500-600A), and finally the device is thermally annealed using nitric oxide gas, and the temperature of the entire process can be 1000-1250 degrees Celsius.

[0114] As a specific example, a saturated doped Dpoly layer (whose thickness may be, for example, 1.5-2um) may be deposited on the outer surface of the fourth gate oxide layer 432, and then the Dpoly layer may be etched back to be flush with the thickness of the fourth gate oxide layer 432. It should be noted that the double polysilicon (D poly, Double Polysilicon) process is a specific semiconductor manufacturing process. The D poly process involves the use of two layers of polysilicon in the manufacturing process of semiconductor devices. The first layer of polysilicon is typically used to form the gate of a transistor, while the second layer of polysilicon is used to make other circuit elements such as interconnects or resistors. The two layers are isolated by an insulating layer.

[0115] In an optional implementation, the step of generating a fourth gate oxide layer 432 at the outermost layer of the current trench 400 includes:

[0116] The third gate oxide layer 431 is etched until the third gate oxide layer 431 is flush with the polysilicon layer 440. Fig.15 As shown;

[0117] A fourth gate oxide layer 432 is grown on an outer surface of the trench 400 , an outer surface of the third gate oxide layer 431 , and an outer surface of the polysilicon layer 440 .

[0118] As a specific example, in this implementation, the third gate oxide layer 431 (ie, SAUSG) may be etched by wet etching until the third gate oxide layer 431 is flush with the polysilicon layer 440 .

[0119] In an optional implementation, after sequentially implanting P-type impurities and N-type impurities into a first region in the top surface of the N-type silicon carbide epitaxial layer 200 and before etching to form a trench 400 in the first region by a photolithography process, the process further includes:

[0120] P-type impurities are implanted into the second region of the top surface to form a second P-type doped region 330, wherein the second P-type doped region 330 is adjacent to both the N-type doped region 310 and the first P-type doped region 320. Fig.16 shown.

[0121] As a specific example, in this implementation, P-type impurities (such as aluminum) can be injected multiple times at high temperatures of 500-600°C with different concentrations, the injection angle can be 0°, the first injection energy can be 30-40kev, and the dose can be 1-5e15 / cm 3 The second implant energy can be 100-200kev and the dose can be 1-5e14 / cm 3 The third implantation energy can be 200-300kev and the dose can be 1-5e14 / cm 3 The fourth implantation energy can be 300-400kev and the dose can be 1-5e14 / cm 3 The fifth implantation energy can be 400-500kev and the dose can be 1-5e15 / cm 3 The sixth implantation energy can be 500-600kev and the dose can be 1-5e14 / cm 3 The seventh implantation energy can be 600-700kev and the dose can be 1-5e13 / cm 3 , and finally a depth of about 3.0um can be formed, with a concentration gradient of 1e18~1e19 / cm 3 The second P-type doping region 330 is formed.

[0122] In an optional implementation, after depositing the second gate oxide layer 460 at the opening of the trench 400 and before growing the source metal layer 461 on the top surface of the second gate oxide layer 460 , the method further includes:

[0123] An ohmic metal layer 510 and a Schottky barrier diode SBD layer 520 are respectively generated in the second region and the third region of the N-type silicon carbide epitaxial layer 200, wherein the third region is adjacent to the second region. Fig.17 shown.

[0124] It can be understood that the conventional silicon carbide trench MOSFET is provided with a P+ / N- junction, the vertical surge voltage is reduced, the reverse recovery charge is reduced, and when the parasitic body diode in the silicon carbide-based integrated SBD and SGT devices is turned on, the junction barrier Schottky diode (JBS) formed by the SBD layer 520 and the epitaxial silicon carbide layer can also prevent the potential failure caused by the conversion of dislocation defects into stacking faults due to the recombination of injected minority carriers. And it does not require any additional process and area loss, which is a cost-effective method.

[0125] In an optional implementation, the step of generating an ohmic metal layer 510 and a Schottky barrier diode SBD layer 520 in the second region and the third region of the N-type silicon carbide epitaxial layer 200 respectively includes:

[0126] An oxide insulating layer 530 is deposited on the third region of the N-type silicon carbide epitaxial layer 200. Fig.18 As shown;

[0127] An ohmic metal layer 510 is deposited on the top surface of the N-type silicon carbide epitaxial layer 200 to form an alloy layer of the ohmic metal layer 510 and silicon carbide. Fig.19 As shown;

[0128] The ohmic metal layer 510 on the surface of the oxide insulating layer 530 and the second gate oxide layer 460 where no alloy is formed is removed. Fig. 20 As shown;

[0129] Etching the oxidized insulating layer 530 and removing the photoresist by a photolithography process to form an SBD generation region;

[0130] sputtering a Schottky metal in the SBD generation region and etching the Schottky metal through a photolithography process;

[0131] The etched Schottky metal is alloyed with silicon carbide to form a SBD layer 520, such as Fig.17 shown.

[0132] Optionally, the deposited oxidized insulating layer 530 in this implementation may be silicon dioxide.

[0133] It should be noted that, in this implementation, after depositing the oxidized insulating layer 530 , it is necessary to etch a hole for the ohmic contact on the oxidized insulating layer 530 .

[0134] In this implementation, as a specific example, an ohmic metal layer 510 (e.g., nickel) 900A-1100A may be deposited on the top surface of the N-type silicon carbide epitaxial layer 200, and a nickel-silicon alloy layer may be formed at 500-700 degrees Celsius, and unalloyed nickel on the surface of the oxide insulating layer 530 and the second gate oxide layer 460 may be further removed by an etching solution, and finally, a high temperature of 900-1000 degrees Celsius may be used for re-alloying to form a good ohmic contact;

[0135] The oxide insulating layer 530 is etched by a photolithography process, the photoresist is removed and then cleaned, a Schottky metal (such as titanium or molybdenum, etc.) is sputtered on the surface, and the Schottky metal is etched by a photolithography process, and the etched Schottky metal is alloyed with a silicon carbide low-temperature alloy to form an SBD junction.

[0136] In an optional implementation, the thickness of the first gate oxide layer 430 is 2000-3000 Å.

[0137] In an optional implementation, the thickness of the polysilicon layer 440 is 5000-6000 Å.

[0138] It can be understood that in the present implementation, the thickness of the polysilicon layer 440 is 5000-6000A, which is approximately two to three times the thickness of the first gate oxide layer 430 (2000-3000A). Thus, since the polysilicon layer 440 is located inside the first gate oxide layer 430, the thickness of the gate oxide layer at the bottom of the trench 400 is finally formed to be 7000-9000A, which is 4 times the original thickness compared to the first gate oxide layer 430 at the bottom of the trench (2000-3000A), thereby effectively improving the device performance.

[0139] In an optional implementation, the thickness of the second gate oxide layer 460 is 500-600 Å.

[0140] It can be understood that in this implementation, the thickness of the second gate oxide layer 460 is 500-600 Å, which can further increase the thickness of the gate oxide layer at the bottom of the trench 400 .

[0141] like Fig.21 The figure shows a structural diagram of a silicon carbide-based integrated SBD and SGT device provided by an embodiment of the present invention, including:

[0142] N-type silicon carbide substrate 100;

[0143] A drain metal layer 300 is sputtered on the back side of the N-type silicon carbide substrate 100;

[0144] An N-type silicon carbide epitaxial layer 200 is grown on the front surface of the N-type silicon carbide substrate 200;

[0145] A first P-type doped region 320 , located inside the N-type silicon carbide epitaxial layer 200 ;

[0146] An N-type doped region 310, located inside the N-type silicon carbide epitaxial layer 200, and between the top surface of the N-type silicon carbide epitaxial layer 200 and the first P-type doped region 420;

[0147] A second P-type doping region 330 is located inside the N-type silicon carbide epitaxial layer 200 and is adjacent to both the N-type doping region 310 and the first P-type doping region 320 ;

[0148] A groove 400 is etched in a first region of the top surface of the N-type silicon carbide epitaxial layer 200 and penetrates the first P-type doped region 320 and the N-type doped region 310;

[0149] A first gate oxide layer 430 is deposited on the outer surface of the trench 400;

[0150] A polysilicon layer 440 is located in the first gate oxide layer 430 and has a metal link hole on the polysilicon layer 440;

[0151] A shielding gate 450 is deposited on the outer surface of the first gate oxide layer 430;

[0152] A second gate oxide layer 460 is deposited at the opening of the trench 400 and covers the opening;

[0153] an ohmic metal layer 510 , adjacent to the second gate oxide layer 460 , and located in a second region of the top surface of the N-type silicon carbide epitaxial layer 200 , the second region being opposite to the second P-type doped region 330 ;

[0154] An SBD metal layer 520 , adjacent to the ohmic metal layer 510 , and formed in a third region of the top surface of the N-type silicon carbide epitaxial layer 200 ;

[0155] The source metal layer 461 covers the SBD metal layer 520 , the ohmic metal layer 510 and the second gate oxide layer 460 .

[0156] In this way, in the silicon carbide-based integrated SBD and SGT devices of the embodiment of the present invention, a polysilicon layer 440 is generated in the first gate oxide layer 430 deposited at the bottom of the trench 400, so that the actual thickness of the first gate oxide layer 430 deposited at the bottom of the trench 400 is the sum of the thickness of the gate oxide layer in the first gate oxide layer 430 and the thickness of the polysilicon layer 440. It can be understood that in this way, compared with the prior art in which there is only a gate oxide layer at the bottom of the trench 400, the thickness of the gate oxide layer at the bottom of the trench 400 of the silicon carbide-based integrated SBD and SGT devices prepared in the embodiment of the present invention is greater than that of the gate oxide layer in the prior art. The thickness can be greatly increased, thereby being able to overcome the problem in the prior art that the gate oxide layer at the two corners of the bottom of the trench is easily broken down due to the excessively high electric field of the gate oxide layer at the bottom of the MOSFET device; in addition, when the thickness of the gate oxide layer in the trench 400 of the trench MOSFET device increases, the gate capacitance will increase, and in the embodiment of the present invention, a polysilicon layer 440 is generated in the first gate oxide layer 430, and a metal link hole is formed on the polysilicon layer 440, and the source metal layer 461 is linked to the polysilicon layer 440 through the metal link hole to achieve the connection between the source and the shielding gate, thereby reducing the gate capacitance. In summary, the embodiment of the present invention can solve the problem in the prior art that the gate oxide layer at the two corners of the bottom of the trench cannot be easily broken down due to the excessively high electric field of the gate oxide layer at the bottom of the MOSFET device when the silicon carbide trench MOSFET device is not used in anti-parallel with a diode;

[0157] It can be understood that the conventional silicon carbide trench MOSFET is provided with a P+ / N- junction, the vertical surge voltage is reduced, the reverse recovery charge is reduced, and when the parasitic body diode in the silicon carbide-based integrated SBD and SGT devices is turned on, the junction barrier Schottky diode (JBS) formed by the SBD layer 520 and the epitaxial silicon carbide layer can also prevent the potential failure caused by the conversion of dislocation defects into stacking faults due to the recombination of injected minority carriers. And it does not require any additional process and area loss, which is a cost-effective method.

[0158] The technical solution provided by the present application is introduced in detail above. The principles and implementation methods of the present application are explained by using specific examples in the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

[0159] Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.

Claims

1. A method for preparing a silicon carbide-based integrated SBD and SGT device, characterized in that: include: Obtaining an N-type silicon carbide substrate, growing an N-type silicon carbide epitaxial layer on the front surface of the N-type silicon carbide substrate, and generating a drain metal layer on the back surface of the N-type silicon carbide substrate; Sequentially implanting P-type impurities and N-type impurities into a first region of the top surface of the N-type silicon carbide epitaxial layer to form adjacent N-type doped regions and a first P-type doped region; Etching a groove in the first region by a photolithography process, wherein the groove passes through the N-type doped region and the first P-type doped region; In the trench, a first gate oxide layer, a polysilicon layer and a shielding gate are sequentially generated from outside to inside, wherein the polysilicon layer is located in the first gate oxide layer; forming a metal link hole on the polysilicon layer; Depositing a second gate oxide layer at the opening of the trench to cover the trench opening; A source metal layer is grown on the top surface of the second gate oxide layer, wherein the source metal layer is connected to the metal link hole.

2. The method for preparing silicon carbide-based integrated SBD and SGT devices according to claim 1, characterized in that: The first gate oxide layer, the polysilicon layer and the shielding gate are sequentially generated from the outside to the inside in the trench, including: A third gate oxide layer is deposited on the bottom and sidewalls of the trench by using a SAUSG method and a SACVD process; Depositing a polysilicon layer on the outer surface of the third gate oxide layer; Etching back the polysilicon layer until the thickness of the polysilicon layer is within a preset range; generating a fourth gate oxide layer at the outermost layer of the trench; In the trench, a D poly layer is deposited on an outer surface of the fourth gate oxide layer to form a shielding gate.

3. The method for preparing silicon carbide-based integrated SBD and SGT devices according to claim 2, characterized in that: The step of generating a fourth gate oxide layer at the outermost layer of the current trench comprises: Etching the third gate oxide layer until the third gate oxide layer is flush with the polysilicon layer; A fourth gate oxide layer is grown on an outer surface of the trench, an outer surface of the third gate oxide layer, and an outer surface of the polysilicon layer.

4. The method for preparing silicon carbide-based integrated SBD and SGT devices according to claim 1, characterized in that: After sequentially implanting P-type impurities and N-type impurities into a first region in the top surface of the N-type silicon carbide epitaxial layer, and before etching to form a groove in the first region by a photolithography process, the method further includes: P-type impurities are implanted into a second region of the top surface to form a second P-type doped region, wherein the second P-type doped region is adjacent to both the N-type doped region and the first P-type doped region.

5. The method for preparing silicon carbide-based integrated SBD and SGT devices according to claim 4, characterized in that: After depositing the second gate oxide layer at the opening of the trench and before growing the source metal layer on the top surface of the second gate oxide layer, the method further includes: An ohmic metal layer and a Schottky barrier diode (SBD) layer are respectively generated in a second region and a third region of the N-type silicon carbide epitaxial layer, wherein the third region is adjacent to the second region.

6. The method for preparing silicon carbide-based integrated SBD and SGT devices according to claim 5, characterized in that: The step of respectively generating an ohmic metal layer and a Schottky barrier diode SBD layer in the second region and the third region of the N-type silicon carbide epitaxial layer comprises: depositing an oxide insulating layer on a third region of the N-type silicon carbide epitaxial layer; Depositing an ohmic metal layer on the top surface of the N-type silicon carbide epitaxial layer to form an alloy layer of the ohmic metal layer and silicon carbide; removing the alloy layer on the surface of the oxide insulating layer and the second gate oxide layer; Etching the oxidized insulating layer and removing the photoresist by a photolithography process to form an SBD generation area; sputtering a Schottky metal in the SBD generation region and etching the Schottky metal through a photolithography process; The etched Schottky metal is alloyed with silicon carbide to form a SBD layer.

7. The method for preparing silicon carbide-based integrated SBD and SGT devices according to claim 1, characterized in that: The thickness of the first gate oxide layer is 2000-3000 Å.

8. The method for preparing silicon carbide-based integrated SBD and SGT devices according to claim 1, characterized in that: The thickness of the polysilicon layer is 5000-6000 Å.

9. The method for preparing silicon carbide-based integrated SBD and SGT devices according to claim 1, characterized in that: The thickness of the second gate oxide layer is 500-600 Å.

10. A silicon carbide-based integrated SBD and SGT device, characterized in that: include: N-type silicon carbide substrate; A drain metal layer is sputtered on the back side of the N-type silicon carbide substrate; An N-type silicon carbide epitaxial layer grown on the front surface of the N-type silicon carbide substrate; A first P-type doped region, located inside the N-type silicon carbide epitaxial layer; an N-type doped region located inside the N-type silicon carbide epitaxial layer and between a top surface of the N-type silicon carbide epitaxial layer and the first P-type doped region; A second P-type doped region, located inside the N-type silicon carbide epitaxial layer, adjacent to both the N-type doped region and the first P-type doped region; A groove is etched in a first region of the top surface of the N-type silicon carbide epitaxial layer and penetrates the first P-type doped region and the N-type doped region; a first gate oxide layer deposited on an outer surface of the trench; A polysilicon layer, located in the first gate oxide layer, and having a metal link hole on the polysilicon layer; A shielding gate, deposited on an outer surface of the first gate oxide layer; A second gate oxide layer is deposited at the opening of the trench and covers the opening; an ohmic metal layer, adjacent to the second gate oxide layer and located in a second region of the top surface of the N-type silicon carbide epitaxial layer, the second region being opposite to the second P-type doped region; an SBD metal layer, adjacent to the ohmic metal layer and formed in a third region of the top surface of the N-type silicon carbide epitaxial layer; The source metal layer covers the SBD metal layer, the ohmic metal layer and the second gate oxide layer.

Citation Information

Cited By

  • Manufacturing method of trench metal oxide semiconductor field effect transistor

    CN121548069A

  • Hardmask modification to enable channeling implantation on silicon carbide devices

    WO2026129349A1