Method for improving SiC / SiO2 interface state density in MOSFET

By using thermal oxidation process and nitrogen gas annealing treatment in SiC oxide semiconductor field effect transistor devices, combined with the passivation effect of trichloroethylene or trichloroethylene, the problem of excessive state density of SiC/SiO2 is solved, and the device is improved carrier channel mobility and reliability.

CN119049973AInactive Publication Date: 2024-11-29吉盛微(武汉)新材料科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411072473.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The SiC oxide semiconductor field effect transistor device has a reduced carrier channel mobility due to the excessive density of SiC/SiO2 interface states, which affects the reliability and service life of the device.

Method used

Thermal oxidation process is used to form a SiO2 gate dielectric layer on the side of the P-type SiC epitaxial layer of the SiC epitaxial sheet away from the N-type SiC substrate, and mix trichloroethylene or trichloroethylene with oxidation gas, and then carry out original operation under a nitrogen gas atmosphere. bit annealing treatment to reduce interfacial state density and repair gate dielectric layer defects.

Benefits of technology

The SiC/SiO2 interface state density is significantly reduced, the interface quality and the density of the SiO2 gate dielectric layer are improved, and the channel mobility of the MOSFET device is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049973A_ABST
    Figure CN119049973A_ABST
Patent Text Reader

Abstract

The invention provides a method for improving SiC / SiO2 interface state density in a metal-oxide-semiconductor field effect transistor (MOSFET), which comprises the following steps of: firstly, providing a SiC epitaxial wafer which comprises an N-type SiC substrate and a P-type SiC epitaxial layer arranged on the N-type SiC substrate; secondly, a SiO2 gate dielectric layer is formed on the side, away from the N-type SiC substrate, of the P-type SiC epitaxial layer through a thermal oxidation process, the gas atmosphere in the thermal oxidation process is mixed gas formed by O2 and first gas, and the first gas is trichloroethylene or trichloroethane; thirdly, in-situ annealing treatment is carried out on the SiO2 gate dielectric layer, and the annealing atmosphere of the in-situ annealing treatment is at least one of N2, N2O and NO; and finally, forming a gate on the surface of one side, far away from the N-type SiC substrate, of the SiO2 gate dielectric layer. According to the method, the SiC / SiO2 interface state density can be obviously reduced, so that the SiC / SiO2 interface quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of microelectronic technology, and in particular to a method for improving SiC / SiO2 interface state density in MOSFET. Background Art

[0002] SiC is currently used to manufacture high-temperature, high-power and high-frequency MOSFETs (Metal-Oxide-Semiconductor Field Effect Transistors) due to its high electron saturation drift velocity, high breakdown electric field and high thermal conductivity. The advantage of SiC is that a dense insulating oxide layer can be formed on the surface of the epitaxial layer through a thermal oxidation process, which serves as the gate dielectric layer of the MOSFET. In the development of SiC oxide semiconductor field effect transistor devices, when the gate dielectric layer of SiO2 material is grown by in-situ thermal oxidation, a SiC / SiO2 interface buffer layer is inevitably formed. Due to the high interface state density and many defects at the SiC / SiO2 interface after thermal oxidation, the lattice mismatch and residual carbon clusters in the buffer layer make the carrier channel mobility of the SiC oxide semiconductor field effect transistor device extremely low, which seriously affects the reliability of the SiC oxide semiconductor field effect transistor device, thereby reducing the service life of the SiC oxide semiconductor field effect transistor device. Summary of the invention

[0003] The purpose of the present invention is to provide a method for improving the SiC / SiO2 interface state density in MOSFET, which is used to improve the technical problem of reduced carrier channel mobility of existing SiC oxide semiconductor field effect transistor devices due to excessively high SiC / SiO2 interface state density.

[0004] In order to solve the above technical problems, the present invention provides a method for improving the SiC / SiO2 interface state density in MOSFET, comprising: S10, providing a SiC epitaxial wafer, wherein the SiC epitaxial wafer includes an N-type SiC substrate and a P-type SiC epitaxial layer disposed on the N-type SiC substrate; S20, forming a SiO2 gate dielectric layer on a side of the P-type SiC epitaxial layer away from the N-type SiC substrate by a thermal oxidation process, wherein the gas atmosphere in the thermal oxidation process is a mixed gas formed by O2 and a first gas, wherein the first gas is trichloroethylene or trichloroethane; S30, performing in-situ annealing on the SiO2 gate dielectric layer, wherein the annealing atmosphere of the in-situ annealing is at least one of N2, N2O and NO; S40, forming a gate on a surface of the SiO2 gate dielectric layer on a side away from the N-type SiC substrate.

[0005] Preferably, in step S10: the thickness of the P-type SiC epitaxial layer is 1-10 μm, and the P-type doping concentration of the P-type SiC epitaxial layer is (1-5)×10 15 cm -3 .

[0006] Preferably, before performing step S20, the method further includes: performing RCA standard wet cleaning on the SiC epitaxial wafer, and soaking the SiC epitaxial wafer in HF solution.

[0007] Preferably, in step S20: the molar ratio of the first gas to O2 is 0.01~0.1.

[0008] Preferably, in step S20: the gas flow rate in the thermal oxidation process is 0.1 to 0.5 L / min.

[0009] Preferably, in step S20, the SiC epitaxial wafer is heated from room temperature to a thermal oxidation temperature and kept warm; the heating rate is 5-10°C / min, the thermal oxidation temperature is 1000-1300°C, and the holding time is 1-5h.

[0010] Preferably, in step S30, the SiC epitaxial wafer is cooled from the thermal oxidation temperature to room temperature by in-situ annealing treatment; the cooling rate of the in-situ annealing treatment is 10-15°C / min, the gas flow rate is 0.5-2L / min, and the annealing time is 1-2h.

[0011] Preferably, the thickness of the SiO2 gate dielectric layer after the in-situ annealing treatment is 20-150 nm.

[0012] Preferably, before performing step S40, the method further comprises: preparing a substrate electrode on a side of the N-type SiC substrate away from the SiO2 gate dielectric layer.

[0013] Preferably, in step S40, the material of the gate is at least one of polysilicon, aluminum, tungsten, titanium, tantalum and molybdenum.

[0014] The beneficial effects of the present invention are as follows: Different from the prior art, the present invention provides a method for improving the SiC / SiO2 interface state density in MOSFET, the method comprising: first, providing a SiC epitaxial wafer, the SiC epitaxial wafer comprising an N-type SiC substrate and a P-type SiC epitaxial layer arranged on the N-type SiC substrate; second, forming a SiO2 gate dielectric layer on a side of the P-type SiC epitaxial layer away from the N-type SiC substrate by a thermal oxidation process, the gas atmosphere in the thermal oxidation process being a mixed gas formed by O2 and a first gas, the first gas being trichloroethylene or trichloroethane; third, performing an in-situ annealing treatment on the SiO2 gate dielectric layer, the annealing atmosphere of the in-situ annealing treatment being at least one of N2, N2O and NO; finally, forming a gate on a surface of the SiO2 gate dielectric layer away from the N-type SiC substrate. The present invention firstly adds trichloroethane or trichloroethylene in the thermal oxidation process, and a passivation effect occurs when chlorine atoms combine with some carbon atoms remaining on the SiC / SiO2 interface during the thermal oxidation process, so that the SiC / SiO2 interface state density is significantly reduced, thereby effectively improving the interface quality of SiC / SiO2; thereafter, the present invention performs an in-situ annealing treatment on the SiO2 gate dielectric layer in a nitrogen-containing gas atmosphere, and N atoms can play a role in passivating the dangling bonds existing at the SiC / SiO2 interface, which is beneficial to further improve the interface quality of SiC / SiO2. At the same time, the fine defects of the SiO2 gate dielectric layer caused by the overflow of gas molecules are repaired by high-temperature annealing, which further improves the compactness of the SiO2 gate dielectric layer and ultimately improves the channel mobility of the prepared MOSFET device. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 A flow chart of a method for improving SiC / SiO2 interface state density in MOSFET provided by an embodiment of the present invention; Figure 2 It is a schematic diagram comparing the SiC oxide semiconductor field effect transistor device prepared in Example 1 of the present invention and the SiC oxide semiconductor field effect transistor device prepared in the comparative example at the SiC / SiO2 interface state density. DETAILED DESCRIPTION

[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] Aiming at the technical problem that the carrier channel mobility of the existing SiC oxide semiconductor field effect transistor device is reduced due to the excessively high SiC / SiO2 interface state density, the present invention can solve the above technical problem.

[0018] See also Figure 1 , Figure 1 A flow chart of a method for improving SiC / SiO2 interface state density in MOSFET provided by an embodiment of the present invention; wherein an embodiment of the present invention provides a method for improving SiC / SiO2 interface state density in MOSFET, comprising: S10, providing a SiC epitaxial wafer, wherein the SiC epitaxial wafer includes an N-type SiC substrate and a P-type SiC epitaxial layer disposed on the N-type SiC substrate.

[0019] Specifically, S10 also includes: First, a SiC epitaxial wafer is provided, wherein the SiC epitaxial wafer includes an N-type SiC substrate and a P-type SiC epitaxial layer disposed on the N-type SiC substrate; The SiC epitaxial wafer is a 6H-SiC wafer; the thickness of the N-type SiC substrate is 1~5μm, the thickness of the P-type SiC epitaxial layer is 1~10μm, and the P-type doping concentration of the P-type SiC epitaxial layer is (1~5)×10 15 cm -3 .

[0020] Specifically, 6H-SiC wafers are hexagonal silicon carbide wafers, which have the following important characteristics and advantages: high thermal conductivity, high hardness, high strength, wide bandgap, good chemical stability and high electron mobility.

[0021] Afterwards, the SiC epitaxial wafer is cleaned using the conventional RCA standard cleaning method and immersed in HF solution; the RCA standard cleaning method plays an important role in semiconductor manufacturing. It can effectively clean the wafer surface and improve the performance and yield of semiconductor devices. The HF solution can remove the natural oxide layer on the surface of the SiC epitaxial wafer.

[0022] Specifically, the method mainly includes the following steps: First, the first standard cleaning solution is used for cleaning, the main components of which are a mixed solution of ammonia (NH3·H2O), hydrogen peroxide (H2O2) and water (H2O). Its function is to remove particles, some metal impurities and organic pollutants.

[0023] Secondly, deionized water is used for rinsing to wash away the chemical substances remaining after the first standard cleaning solution is used for cleaning.

[0024] Next, the second standard cleaning solution is used for cleaning, the main components of which are a mixed solution of hydrochloric acid (HCl), hydrogen peroxide (H2O2) and water (H2O). Its function is to remove impurities such as metal ions.

[0025] Finally, deionized water is continued to be used for rinsing to thoroughly clean the residual chemicals on the SiC epitaxial wafer.

[0026] S20, forming a SiO2 gate dielectric layer on a side of the P-type SiC epitaxial layer away from the N-type SiC substrate by a thermal oxidation process, wherein the gas atmosphere in the thermal oxidation process is a mixed gas formed by O2 and a first gas, and the first gas is trichloroethylene or trichloroethane.

[0027] Specifically, S20 also includes: The cleaned SiC epitaxial wafer is directly placed in an oxidation furnace for thermal oxidation reaction to generate a SiO2 gate dielectric layer; wherein the SiO2 gate dielectric layer is located on the side of the P-type SiC epitaxial layer away from the N-type SiC substrate; the gas atmosphere in the thermal oxidation process is a mixed gas formed by O2 and a first gas, and the first gas is trichloroethylene or trichloroethane.

[0028] In this step, trichloroethane or trichloroethylene gas is added to the thermal oxidation reaction to improve the interface quality of SiC / SiO2, so that the interface state density and oxide charge density are significantly reduced, as follows: (1) The passivation effect occurs when chlorine combines with residual carbon atoms remaining on the SiC / SiO2 interface during the oxidation process; (2) Trichloroethane or trichloroethylene produces almost no additional carbon during the oxidation process, because CO2 is easily formed in an O2-rich environment, and no additional interface states and oxide charges are generated; (3) The Cl2 or HCl produced by the reaction system has an absorption effect on ion contamination from SiC dopants and oxidative systems that diffuse outward, which is particularly important in P-type wafers and will lead to a reduction in oxide charge.

[0029] Preferably, in step S20: the molar ratio of the first gas to O2 is 0.01-0.1; from the perspective of reaction control, this ratio range can ensure that chlorine plays an appropriate role in the oxidation process, which can achieve positive effects such as effective passivation of residual carbon atoms, and will not cause other unnecessary side reactions or negatively affect material properties due to excessive chlorine content. If the ratio is too low, the role of chlorine may not be fully utilized to improve the interface quality; and if the ratio is too high, it may bring some unknown adverse effects, such as excessive modification or potential damage to the material structure or performance.

[0030] Preferably, in step S20: the gas flow rate in the thermal oxidation process is 0.1 to 0.5 L / min.

[0031] From the perspective of reaction uniformity, a suitable gas flow rate can ensure that the gas is evenly distributed in the oxidation furnace, so that all parts of the SiC epitaxial wafer can undergo thermal oxidation reactions more evenly, avoiding insufficient or excessive local reactions, thereby helping to obtain a uniform SiO2 gate dielectric layer. If the flow rate is too low, it may lead to uneven gas distribution and insufficient reaction in some areas; while if the flow rate is too high, the reaction may be too intense or difficult to control, and may also bring some unstable factors.

[0032] Preferably, in step S20, the SiC epitaxial wafer is heated from room temperature to a thermal oxidation temperature and kept warm; the heating rate is 5-10°C / min, the thermal oxidation temperature is 1000-1300°C, and the holding time is 1-5h.

[0033] Among them, the heating rate is 5 to 10℃ / min, which is a moderate heating rate. If the heating rate is too fast, the SiC epitaxial wafer may be damaged by cracking due to the rapid accumulation of thermal stress; if the heating rate is too slow, the process time may be extended and production efficiency may be reduced; the thermal oxidation temperature is selected to be 1000~1300℃, because this temperature range can better promote the oxidation reaction, while the temperature will not be too high to cause excessive thermal damage to the material or other adverse effects; the holding time is set to 1~5h, which is to ensure that the oxidation reaction is fully carried out and the SiO2 gate dielectric layer reaches sufficient thickness and quality. If the holding time is too short, the oxidation may not be complete, affecting the performance of the gate dielectric layer; if the time is too long, it may increase energy consumption and time costs, and may not necessarily lead to further significant quality improvements.

[0034] S30, performing in-situ annealing on the SiO2 gate dielectric layer, wherein the annealing atmosphere of the in-situ annealing is at least one of N2, N2O and NO.

[0035] Specifically, S30 also includes: The SiC epitaxial wafer is subjected to in-situ annealing treatment, and the annealing atmosphere of the in-situ annealing treatment is at least one of N2, N2O and NO; wherein the SiC epitaxial wafer is cooled from the thermal oxidation temperature to the room temperature through the in-situ annealing treatment; the cooling rate of the in-situ annealing treatment is 10-15°C / min, the gas flow rate is 0.5-2L / min, and the annealing time is 1-2h. At this time, the thickness of the SiO2 gate dielectric layer after the in-situ annealing treatment is 20-150nm.

[0036] Specifically, after the thermal oxidation is completed, the SiC epitaxial wafer continues to be annealed in situ under the atmosphere of NO, N2O, and N2 for 1 to 2 hours. When SiO2 is formed by thermal oxidation, excess C will be generated to form C clusters. After rapid annealing, O can react with C at the interface and release in the form of CO, thereby reducing the density of C clusters to a certain extent. At the same time, N plays a role in passivating the Si hanging bonds generated at the SiC / SiO2 interface, which is beneficial to improving the interface quality. At the same time, the fine defects in the SiO2 gate dielectric layer caused by the overflow of gas molecules are repaired by high-temperature annealing, which improves the density of the SiO2 gate dielectric layer film.

[0037] Afterwards, after the in-situ annealing of the SiO2 gate dielectric layer is completed, a substrate electrode is prepared on the side of the N-type SiC substrate away from the SiO2 gate dielectric layer. The specific process is as follows: the SiO2 gate dielectric layer after the in-situ annealing is placed in a DC sputtering chamber, and an Al substrate electrode is prepared by atomic deposition.

[0038] S40, forming a gate on a surface of the SiO2 gate dielectric layer on a side away from the N-type SiC substrate.

[0039] Specifically, step S40 also includes: A gate is formed on a surface of a SiO2 gate dielectric layer away from an N-type SiC substrate by using a photolithography process. The gate material is at least one of polysilicon, aluminum, tungsten, titanium, tantalum and molybdenum.

[0040] The technical solution of the present invention is now further described in conjunction with specific embodiments.

[0041] Embodiment 1: This embodiment 1 provides a method for improving the SiC / SiO2 interface state density in MOSFET, and the specific implementation steps include: Step 1: Provide a SiC epitaxial wafer, wherein the SiC epitaxial wafer comprises an N-type SiC substrate and a P-type SiC epitaxial layer disposed on the N-type SiC substrate; wherein the SiC epitaxial wafer is a (0001) Si surface 6H-SiC wafer, the epitaxial layer grown on the SiC wafer substrate has a thickness of 5 μm, and the doping concentration of the epitaxial layer is 4×10 15 cm -3 .

[0042] Step 2, using a conventional RCA standard cleaning method to clean the SiC epitaxial wafer, including: (1) soaking the SiC epitaxial wafer in toluene, acetone, and ethanol in order for 30 minutes; (2) transferring the SiC epitaxial wafer to a mixed solution of H2O and H2SO4 with a molar ratio of 1:1 and soaking it for 15 minutes; (3) placing the SiC epitaxial wafer in concentrated H2SO4 with a mass fraction of more than 98% and boiling it until a large amount of white smoke is emitted; (4) transferring the SiC epitaxial wafer to a HF solution with a mass fraction of 0.5% and soaking it for 1 minute; (5) transferring the SiC epitaxial wafer to standard solution No. 1 (the mass ratio of H2O: H2O2: NH3·H2O is 5:1:1) and soaking it at 80°C for 15 minutes; (6) transferring the SiC epitaxial wafer to standard solution No. 2 (the mass ratio of H2O: H2O2: HCl is 6:1:1) and soaking it at 80°C for 15 minutes; a large amount of hot and cold deionized water is used for rinsing between the above steps.

[0043] Step three, load the cleaned SiC epitaxial wafer into an oxidation furnace, introduce 250 ml / min of a mixed gas of O2 and trichloroethylene or trichloroethane into the reaction chamber, the molar ratio of trichloroethylene or trichloroethane to O2 is 0.05, and heat from room temperature (25°C) to 1200°C at 10°C / min for thermal oxidation reaction, and keep warm for 5 hours.

[0044] Step 4. After oxidation, an in-situ annealing treatment is performed for 2 hours in a mixed atmosphere of N2, N2O, and NO (the volume ratio of N2:N2O:NO is 2:1:1) at the same temperature with a gas flow rate of 1L / min, and then the temperature is reduced from 1200°C to room temperature (25°C) at a cooling rate of 10°C / min to finally complete the preparation of the SiO2 gate dielectric layer. The thickness of the SiO2 gate dielectric layer is 134nm.

[0045] Step 5: forming a gate on the surface of the SiO2 gate dielectric layer away from the N-type SiC substrate. The gate is made of molybdenum and has a thickness of 50 nm.

[0046] Comparative Example 1: Comparative Example 1: A SiC oxide semiconductor field effect transistor device is prepared by a conventional method, and the specific preparation steps are as follows: Step 1: Provide a SiC epitaxial wafer, wherein the SiC epitaxial wafer comprises an N-type SiC substrate and a P-type SiC epitaxial layer disposed on the N-type SiC substrate; wherein the SiC epitaxial wafer is a (0001) Si surface 6H-SiC wafer, the epitaxial layer grown on the SiC wafer substrate has a thickness of 5 μm, and the doping concentration of the epitaxial layer is 4×10 15 cm -3 .

[0047] Step 2, cleaning the SiC epitaxial wafer using a conventional RCA standard cleaning method, including: (1) soaking the SiC epitaxial wafer in toluene, acetone, and ethanol in order for 30 minutes; (2) transferring the SiC epitaxial wafer to a mixed solution of H2O and H2SO4 with a molar ratio of 1:1 and soaking it for 15 minutes; (3) placing the SiC epitaxial wafer in concentrated H2SO4 with a mass fraction of more than 98% and boiling it until a large amount of white smoke is emitted; (4) transferring the SiC epitaxial wafer to a HF solution with a mass fraction of 0.5% and soaking it for 1 minute; (5) transferring the SiC epitaxial wafer to standard solution No. 1 (the mass ratio of H2O: H2O2: NH3·H2O is 5:1:1) and soaking it at 80°C for 15 minutes; (6) transferring the SiC epitaxial wafer to standard solution No. 2 (the mass ratio of H2O: H2O2: HCl is 6:1:1) and soaking it at 80°C for 15 minutes; a large amount of hot and cold deionized water is used for rinsing between the above steps.

[0048] Step 3: Place the cleaned SiC epitaxial wafer into an oxidation furnace, introduce 250 ml / min of O2 into the reaction chamber, and heat the reaction from room temperature (25°C) to 1200°C at a rate of 10°C / min for a thermal oxidation reaction, with a holding time of 5 hours.

[0049] Step 4: After oxidation, the temperature is lowered from 1200° C. to room temperature (25° C.) at a cooling rate of 10° C. / min, and finally the preparation of the SiO 2 gate dielectric layer is completed. The thickness of the SiO 2 gate dielectric layer is 117 nm.

[0050] Step 5: forming a gate on the surface of the SiO2 gate dielectric layer away from the N-type SiC substrate. The gate is made of molybdenum and has a thickness of 50 nm.

[0051] See also Figure 2 , Figure 2 Schematic diagram showing the comparison of the SiC oxide semiconductor field effect transistor device prepared in Example 1 of the present invention and the comparative example at the SiC / SiO2 interface state density; wherein the abscissa is the interface state energy Ec-E t (Ev), the ordinate is the interface state density Dit (cm -2 eV -1 ), the hollow part is the thermal oxidation reaction of the comparative example under an O2 atmosphere, and the solid part is the thermal oxidation reaction of Example 1 under a trichloroethylene (TCE) atmosphere.

[0052] Specifically, by Figure 2It can be seen that the SiC / SiO2 interface state density in Example 1 of the present invention is significantly reduced compared with that in Comparative Example 1; in addition, the thickness of the SiO2 gate dielectric layer prepared in Example 1 of the present invention is 134nm, while the thickness of the SiO2 gate dielectric layer prepared in Comparative Example 1 is 117nm, which indicates that the method for improving the SiC / SiO2 interface state density in MOSFET provided by Example 1 of the present invention has improved oxidation efficiency in the thermal oxidation process compared with the preparation method provided by Comparative Example 1.

[0053] In summary, different from the prior art, the present invention provides a method for improving the SiC / SiO2 interface state density in MOSFET, the method comprising: first, providing a SiC epitaxial wafer, the SiC epitaxial wafer comprising an N-type SiC substrate and a P-type SiC epitaxial layer arranged on the N-type SiC substrate; second, forming a SiO2 gate dielectric layer on a side of the P-type SiC epitaxial layer away from the N-type SiC substrate by a thermal oxidation process, the gas atmosphere in the thermal oxidation process is a mixed gas formed by O2 and a first gas, the first gas is trichloroethylene or trichloroethane; third, performing an in-situ annealing treatment on the SiO2 gate dielectric layer, the annealing atmosphere of the in-situ annealing treatment is at least one of N2, N2O and NO; finally, forming a gate on a surface of the SiO2 gate dielectric layer away from the N-type SiC substrate. The present invention firstly adds trichloroethane or trichloroethylene in the thermal oxidation process, and a passivation effect occurs when chlorine atoms combine with some carbon atoms remaining on the SiC / SiO2 interface during the thermal oxidation process, so that the SiC / SiO2 interface state density is significantly reduced, thereby effectively improving the interface quality of SiC / SiO2; thereafter, the present invention performs an in-situ annealing treatment on the SiO2 gate dielectric layer in a nitrogen-containing gas atmosphere, and N atoms can play a role in passivating the dangling bonds existing at the SiC / SiO2 interface, which is beneficial to further improve the interface quality of SiC / SiO2. At the same time, the fine defects of the SiO2 gate dielectric layer caused by the overflow of gas molecules are repaired by high-temperature annealing, which further improves the compactness of the SiO2 gate dielectric layer and ultimately improves the channel mobility of the prepared MOSFET device.

[0054] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.

[0055] The above embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for improving SiC / SiO2 interface state density in MOSFET, characterized in that: include: S10, providing a SiC epitaxial wafer, wherein the SiC epitaxial wafer comprises an N-type SiC substrate and a P-type SiC epitaxial layer disposed on the N-type SiC substrate; S20, forming a SiO2 gate dielectric layer on a side of the P-type SiC epitaxial layer away from the N-type SiC substrate by a thermal oxidation process, wherein the gas atmosphere in the thermal oxidation process is a mixed gas formed by O2 and a first gas, wherein the first gas is trichloroethylene or trichloroethane; S30, performing an in-situ annealing treatment on the SiO2 gate dielectric layer, wherein the annealing atmosphere of the in-situ annealing treatment is at least one of N2, N2O and NO; S40, forming a gate on a surface of the SiO2 gate dielectric layer on a side away from the N-type SiC substrate.

2. The method for improving SiC / SiO2 interface state density in MOSFET according to claim 1, characterized in that: In the step S10, the thickness of the P-type SiC epitaxial layer is 1-10 μm, and the P-type doping concentration of the P-type SiC epitaxial layer is (1-5)×10 15 cm -3 .

3. The method for improving SiC / SiO2 interface state density in MOSFET according to claim 1, characterized in that: Before performing the step S20, the method further includes: performing a standard wet cleaning process on the SiC epitaxial wafer, and soaking the SiC epitaxial wafer in an HF solution.

4. The method for improving SiC / SiO2 interface state density in MOSFET according to claim 1, characterized in that: In the step S20: the molar ratio of the first gas to O2 is 0.01-0.

1.

5. The method for improving SiC / SiO2 interface state density in MOSFET according to claim 1, characterized in that: In the step S20: the gas flow rate in the thermal oxidation process is 0.1 to 0.5 L / min.

6. The method for improving SiC / SiO2 interface state density in MOSFET according to claim 1, characterized in that: In the step S20, the SiC epitaxial wafer is heated from room temperature to a thermal oxidation temperature and kept warm; the heating rate is 5-10°C / min, the thermal oxidation temperature is 1000-1300°C, and the holding time is 1-5h.

7. The method for improving SiC / SiO2 interface state density in MOSFET according to claim 1, characterized in that: In the step S30, the SiC epitaxial wafer is cooled from the thermal oxidation temperature to the room temperature by the in-situ annealing treatment; the cooling rate of the in-situ annealing treatment is 10-15°C / min, the gas flow rate is 0.5-2L / min, and the annealing time is 1-2h.

8. The method for improving SiC / SiO2 interface state density in MOSFET according to claim 1, characterized in that: The thickness of the SiO2 gate dielectric layer after the in-situ annealing treatment is 20-150 nm.

9. The method for improving SiC / SiO2 interface state density in MOSFET according to claim 1, characterized in that: Before performing the step S40, the method further includes: preparing a substrate electrode on a side of the N-type SiC substrate away from the SiO2 gate dielectric layer.

10. The method for improving SiC / SiO2 interface state density in MOSFET according to claim 1, characterized in that: In the step S40, the material of the gate is at least one of polysilicon, aluminum, tungsten, titanium, tantalum and molybdenum.

Citation Information

Patent Citations

  • Method for improving SiC and SiO2 interface state density

    CN104966665A

  • Method of fabricating an oxide layer on a silicon carbide layer utilizing n¿2?o

    WO2002029874A2