Nanorod array-nanowire net-shaped heterojunction structure material growing on FTO substrate and preparation method and application of nanorod array-nanowire net-shaped heterojunction structure material
By preparing the CdS-Bi2S3 material with nanorod array-nanowire mesh heterojunction structure on the FTO substrate under a hydrothermal solvent-heat system, the lack of morphological diversity of cadmium sulfide and bismuth sulfide nanomaterials in the prior art is solved. The problem of this problem achieves efficient photodetection performance and broadband response.
Patent Information
- Application Number
- CN202411076981.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art is difficult to meet the increasing demands of modern use, and it is impossible to effectively prepare cadmium sulfide and bismuth sulfide nanomaterials with diverse morphology, especially in the application of photodetectors and solar cells.
The CdS-Bi2S3 material with nanorod array-nanowire mesh heterojunction structure was prepared by using FTO substrate under a hydrothermal solvent-heating system through autoclave heating reaction. The CdS-Bi2S3 material with nanorod array-nanowire mesh heterojunction structure was prepared using thiourea, cadmium source and surfactant. Step-by-step growth was carried out under conditions to form a uniform nanorod array and nanowire mesh structure.
Achieve low-cost and simple preparation of nanorod array-nanowire mesh heterojunction structures with uniform morphology, improve light absorption efficiency and carrier migration path, widen the spectral effect range, and is suitable for broadband in the field of photoelectric detection. response.
Smart Images

Figure CN119050197A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor materials and inorganic compound nanomaterials, and in particular to a nanorod array-nanowire mesh heterojunction structure material grown on an FTO substrate, and a preparation method and application thereof. Background Art
[0002] Cadmium sulfide-based nanomaterials are one of the most widely used optoelectronic materials. Their ideal direct band gap and suitable band edge position make them one of the most promising semiconductor materials in the fields of photodetectors, photocatalysis and solar cells.
[0003] Bismuth sulfide has an excellent light absorption coefficient, and its nanomaterials have excellent flexibility and mechanical stability, and have great application prospects in photoelectric detection including wearable electronic devices.
[0004] However, the cadmium sulfide and bismuth sulfide prepared by the prior art cannot meet the increasingly high requirements of modern use. The prior art prepares them by composite method, for example:
[0005] The patent with publication number CN 105513805 A published on April 20, 2016 discloses copper-cadmium-germanium-sulfur nanocrystals, copper-cadmium-germanium-sulfur counter electrodes, and preparation methods and applications thereof. The copper-cadmium-germanium-sulfur nanocrystals disclosed herein have a molar ratio of copper, cadmium, germanium and sulfur of (2-2.2):(1-1.2):(1-1.2):(4-4.2), and the preparation of the copper-cadmium-germanium-sulfur counter electrode is achieved by coating copper-cadmium-germanium-sulfur nano-ink on a conductive substrate. The copper-cadmium-germanium-sulfur nanocrystals are synthesized by a low-temperature liquid phase method, have an orthorhombic crystal system, and are a supercell structure derived from wurtzite, with the advantages of uniform size, high crystallinity, and good monodispersity. When used as a counter electrode catalyst for dye-sensitized solar cells, the I3 - The reduction of ions shows good catalytic activity. The product prepared is nanocrystalline, and the preparation method of products with other morphologies is not disclosed. Summary of the invention
[0006] The purpose of the present invention is to provide a nanorod array-nanowire network heterojunction structure material grown on a FTO substrate and a preparation method thereof, and to prepare the nanorod array-nanowire network heterojunction structure simply and at low cost under a hydrothermal solvent thermal system.
[0007] Another object of the present invention is to provide a nanorod array-nanowire network heterojunction structure material grown on a FTO substrate for use in the field of photoelectric detection.
[0008] The specific technical solutions of the present invention are as follows:
[0009] A method for preparing a nanorod array-nanowire network heterojunction structure material grown on a FTO substrate comprises the following steps:
[0010] 1) placing the FTO glass in an autoclave containing a sulfur source, a cadmium source, a surfactant and water, heating the autoclave to react, and obtaining a CdS nanorod array material grown on the FTO substrate;
[0011] 2) The CdS nanorod array material grown on the FTO substrate prepared in step 1) is placed in an autoclave containing a sulfur source, a bismuth source and ethylene glycol, and heated to react to obtain a CdS-Bi2S3 nanorod array-nanowire network heterojunction structure material grown on the FTO substrate.
[0012] In step 1), the molar ratio of the sulfur source, the cadmium source and the surfactant is 0.3-0.9:0.1-0.3:0.06-0.2;
[0013] In step 1), the usage ratio of the cadmium source and water is 0.0025-0.015 mol / L;
[0014] In step 1), the sulfur source is thiourea;
[0015] In step 1), the cadmium source is cadmium nitrate tetrahydrate;
[0016] In step 1), the surfactant is glutathione;
[0017] In step 1), the FTO glass is placed in an autoclave with the conductive surface facing downward.
[0018] In step 1), the temperature of the deionized water used is room temperature, 25°C;
[0019] In step 1), the FTO glass is fluorine-doped SnO2 conductive glass;
[0020] In step 1), the heating reaction refers to: reacting at 180-200° C. for 2-4 hours;
[0021] Step 1) After the reaction is completed, the FTO glass sample is rinsed with deionized water and ethanol, and placed in a vacuum oven for drying;
[0022] In step 2), the molar ratio of the sulfur source to the bismuth source is 0.3-0.6:0.2-0.4;
[0023] In step 2), the dosage ratio of the bismuth source to ethylene glycol is 0.0055-0.016 mol / L;
[0024] The molar ratio of the cadmium source in step 1) to the bismuth source in step 2) is 0.1-0.3:0.2-0.4;
[0025] In step 2), the temperature of the ethylene glycol is room temperature, 25°C;
[0026] In step 2), the sulfur source is thiourea;
[0027] In step 2), the bismuth source is bismuth nitrate pentahydrate;
[0028] In step 2), the heating reaction refers to: reacting at 60-80° C. for 18-24 hours;
[0029] After the reaction in step 2) is completed, the FTO glass sample is rinsed with deionized water and ethanol, and placed in a vacuum oven for drying to obtain a CdS-Bi2S3 nanorod array-nanowire network heterojunction structure grown on the FTO substrate.
[0030] Preferably, the method for preparing the nanorod array-nanowire network heterojunction structure material grown on the FTO substrate comprises the following steps:
[0031] 1) The FTO glass is ultrasonically cleaned with acetone, ethanol and water in sequence, and placed in an oven for drying; thiourea, glutathione, cadmium nitrate tetrahydrate and water are weighed in sequence and placed in a polytetrafluoroethylene liner, and a mixed solution is obtained by ultrasonic treatment; the cleaned and dried FTO glass is placed with the conductive surface facing downward into the mixed solution; the reactor is assembled and reacted at 180-200°C for 2-4h; after the reaction is completed, the FTO glass sample is rinsed with deionized water and ethanol, and placed in a vacuum oven for drying;
[0032] 2) Weighing thiourea, bismuth nitrate pentahydrate and ethylene glycol and putting them into a polytetrafluoroethylene liner, and ultrasonically obtaining a mixed solution; placing the side on which the CdS nanorod array is grown in step 1) face down into the mixed solution; assembling the reaction kettle, and reacting at 60-80° C. for 18-24 hours; after the reaction, rinsing the FTO glass sample with deionized water and ethanol, and putting it into a vacuum oven for drying, thereby obtaining a CdS-Bi2S3 nanorod array-nanowire network heterojunction structure grown on the FTO substrate.
[0033] In the reaction system of the present invention, firstly, a sulfur source and a cadmium source are placed under high temperature and high pressure in a polytetrafluoroethylene-lined stainless steel autoclave, so that tiny CdS crystal nuclei are rapidly generated on an FTO substrate, and the crystal nuclei grow along a single direction on the FTO surface. Simultaneously, under the action of a surfactant, glutathione, a CdS nanorod array with a vertical structure grows in a single direction, and the morphology is uniform and not agglomerated. Then, after the sulfur source and the bismuth source are loaded with growth under high temperature and high pressure in a polytetrafluoroethylene-lined stainless steel autoclave, the used ethylene glycol has higher viscosity, and the size grown under high temperature and high pressure is more suitable to form a network structure with the CdS nanorods, so that a CdS-Bi2S3 nanorod array-nanowire network heterojunction structure grown on the FTO substrate is finally obtained.
[0034] The invention provides a nanorod array-nanowire mesh heterojunction structure material grown on an FTO substrate, which is prepared by the above method. The product is: a CdS-Bi2S3 nanorod array-nanowire mesh heterojunction structure grown on an FTO substrate, the nanorod size is 100-200nm, the nanowire size is 5-10nm, and the mesh is interwoven to form a special heterojunction with uniform size.
[0035] The product obtained by the present invention can be directly used for the assembly and performance research of optoelectronic devices. The X-ray diffraction data of the sample are analyzed, and the seven characteristic peaks of diffraction peaks at 24.83°, 26.54°, 28.22°, 36.66°, 43.74°, 47.89° and 51.89° respectively correspond to the (100), (002), (101), (102), (110), (103) and (112) crystal planes of CdS (01-077-2306). After Bi2S3 is loaded, the CdS / Bi2S3 heterojunction has five obvious characteristic peaks at 15.65°, 17.55°, 31.74°, 39.84° and 45.40°, which respectively correspond to the (020), (120), (221), (141) and (002) crystal planes of Bi2S3. This indicates that two simple components were successfully synthesized with good crystallinity.
[0036] The present invention provides an application of a nanorod array-nanowire mesh heterojunction structure material grown on a FTO substrate, which is used in the field of photoelectric detection, especially broadband response, near-ultraviolet to infrared broadband photoelectric detectors. The present invention tested the photoelectric performance of the synthesized CdS-Bi2S3 nanorod array-nanowire mesh heterojunction structure device, and the results showed that the construction of the heterojunction material has great potential in the field of photoelectric detection.
[0037] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention adopts a simple hydrothermal solvent thermal system of a reactor to prepare a uniformly grown mesh CdS-Bi2S3 nanorod array-nanowire heterojunction structure on an FTO substrate, which is easy to operate and does not require complicated steps. The device can be directly used for the assembly and performance research of optoelectronic devices. The nanorod array-nanowire mesh heterojunction structure grown on the FTO substrate has a special vertical structure, which is conducive to carrier migration. At the same time, the special mesh heterojunction structure greatly improves the light absorption efficiency, inhibits carrier recombination, and broadens the spectral effect range. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 is a scanning electron microscope image of the CdS-Bi2S3 nanorod array-nanowire network heterojunction structure obtained in Example 1;
[0039] Figure 2is a scanning electron microscope image of the CdS nanorod array obtained in Example 2;
[0040] Figure 3 is an XRD pattern of the CdS-Bi2S3 nanorod array-nanowire network heterojunction structure and the obtained CdS nanorod array obtained in Comparative Example 1 and Example 2;
[0041] Figure 4 is the X-ray photoelectron spectrum of the product obtained in Example 1;
[0042] Figure 5 This is a photo of the photoelectric device obtained in Example 1;
[0043] Figure 6 1 is an IV diagram of the photoelectric devices obtained by comparing Example 1 and Example 2 under light sources of different excitation wavelengths at a fixed power;
[0044] Figure 7 is an IT diagram obtained by periodically switching the light source on and off the photoelectric device obtained by comparing Example 1 and Example 2;
[0045] Figure 8 is a graph comparing the photocurrent and light power intensity of the photoelectric devices obtained in Example 1 and Example 2 under a light source with a fixed excitation wavelength;
[0046] Fig. 9 Comparison of the responsivity R and the detection rate D of the photoelectric devices obtained in Example 1 and Example 2 under light sources of different excitation wavelengths;
[0047] Fig.10 1 is an IT diagram of the optoelectronic device obtained in Example 1 at different powers under light sources with excitation wavelengths of 405 nm, 520 nm, and 1060 nm;
[0048] Fig.11 is a scanning electron microscope image of the CdS-Bi2S3 nanorod array-nanowire network heterojunction structure obtained in Example 3;
[0049] Fig.12 is an IT diagram obtained by periodically switching the light source on and off the photoelectric device obtained in Example 3;
[0050] Fig.13 is a scanning electron microscope image of the CdS-Bi2S3 nanorod array-nanowire network heterojunction structure obtained in Example 4;
[0051] Fig.14 This is an IT diagram obtained by periodically switching the light source of the photoelectric device obtained in Example 4. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0054] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0055] The FTO glass used in the present invention is fluorine-doped SnO2 conductive glass, the manufacturer is Zhuhai Kaiwei Optoelectronics Technology, the model is KV-FTO-R15T22-100100, the parameter is 14-16ohm / sg, the size is 1-10×1-10×10-100mm, and before use, it is ultrasonically cleaned with acetone, ethanol and water in turn, and placed in an oven for drying.
[0056] Example 1
[0057] A method for preparing a nanorod array-nanowire network heterojunction structure material grown on a FTO substrate comprises the following steps:
[0058] 1) Weigh 0.9mmol of thiourea, 0.18mmol of glutathione and 0.3mmol of cadmium nitrate tetrahydrate respectively and put them into a polytetrafluoroethylene liner, add 30mL of deionized water, and ultrasonicate to obtain a mixed solution. Put the washed and dried FTO glass with the conductive surface facing down, install a stainless steel autoclave, heat it to 200℃, and react for 4h under high temperature and high pressure and the action of surfactant glutathione. After the reaction is completed, take out the FTO glass sample, rinse it with deionized water and ethanol, and dry it in a vacuum oven to obtain a glass sample of CdS nanorod array grown on FTO substrate.
[0059] 2) Then weigh 0.3mmol bismuth nitrate pentahydrate and 0.3mmol thiourea, put them into a polytetrafluoroethylene liner, add 30mL ethylene glycol, ultrasonically obtain a mixed solution, put the FTO glass sample, put the sample face down, install the stainless steel autoclave, heat it to 60℃, and react for 24h. After the reaction, take out the FTO glass sample, rinse it with deionized water and ethanol, and obtain a glass sample with a nanorod array-nanowire network heterojunction structure grown on the FTO substrate.
[0060] The application of the nanorod array-nanowire network heterojunction structure material grown on the FTO substrate prepared in Example 1 in a photodetector is specifically as follows:
[0061] The back of the glass sample was glued to the PCB board containing copper foil with silver paste, and then the conductive silver paste was dripped on the graphene surface and FTO substrate respectively, and high-purity silver wire was used as an external circuit connection. In this way, a simple device model of the photodetector can be made.
[0062] Example 2 (Step 1 of Example 1)
[0063] A method for preparing a nanorod array grown on a FTO substrate comprises the following steps:
[0064] Weigh 0.9mmol of thiourea, 0.18mmol of glutathione and 0.3mmol of cadmium nitrate tetrahydrate respectively and put them into a polytetrafluoroethylene liner, add 30mL of deionized water, and ultrasonicate to obtain a mixed solution. Put the washed and dried FTO glass with the conductive surface facing down, install a stainless steel autoclave, heat it to 200℃, and react for 4 hours under high temperature, high pressure and surfactant. After the reaction is completed, take out the FTO glass sample, rinse it with deionized water and ethanol, and obtain a glass sample of CdS nanorod array grown on FTO substrate.
[0065] The application of the material prepared in Example 2 in a photoelectric detector is specifically as follows:
[0066] The back of the glass sample was glued to the PCB board containing copper foil with silver paste, and then the conductive silver paste was dripped on the graphene surface and FTO substrate respectively, and high-purity silver wire was used as an external circuit connection. In this way, a simple device model of the photodetector can be made.
[0067] Figure 1 This is a scanning electron microscope image of the CdS-Bi2S3 nanorod array-nanowire network heterojunction structure obtained in Example 1. The network heterojunction structure can be clearly seen from the image.
[0068] Figure 2 This is a scanning electron microscope image of the CdS nanorod array obtained in Example 2. From the image, it can be seen that the nanorod array has an obvious vertical structure.
[0069] Figure 3The XRD patterns of the CdS-Bi2S3 nanorod array-nanowire network heterojunction structure and the obtained CdS nanorod array obtained in Comparative Example 1 and Example 2. Compared with the standard card, the seven characteristic peaks of diffraction peaks at 24.83°, 26.54°, 28.22°, 36.66°, 43.74°, 47.89° and 51.89° correspond to the (100), (002), (101), (102), (110), (103) and (112) crystal planes of CdS (01-077-2306), respectively, which indicates that the CdS nanorod array was successfully synthesized. After loading Bi2S3, the CdS / Bi2S3 heterojunction has five obvious characteristic peaks at 15.65°, 17.55°, 31.74°, 39.84° and 45.40°, corresponding to the (020), (120), (221), (141) and (002) crystal planes of Bi2S3, respectively. This indicates that the CdS / Bi2S3 heterojunction structure has been successfully synthesized with good crystallinity.
[0070] Figure 4 This is the X-ray photoelectron spectrum of the product obtained in Example 1. The S2p, Cd3d and Bi 4f energy level spectra are calibrated with C1s (284.80 eV). It can be seen Figure 4 The two peaks at 411.83 and 405.08 eV belong to Cd 3d 3 / 2 and Cd3d 5 / 2 , the double peak spacing is 6.75 eV, indicating the presence of Cd 2+ At the same time, S 2- The characteristic peak of 160.56 eV (S2p 3 / 2 ) and 161.54eV(S2p 1 / 2 The two peaks at 163.50 and 158.30 eV belong to Bi 4f 5 / 2 and Bi 4f 7 / 2 , the double peak distance of 5.20 eV indicates that Bi 3+ The results of X-ray photoelectron spectroscopy are highly consistent with the XRD results, indicating that the synthesis method of the present invention is used to successfully prepare the CdS-Bi2S3 nanorod array-nanowire network heterojunction structure.
[0071] Figure 5 This is a photo of the photoelectric device obtained in Example 1. The photoelectric device can be connected to the photoelectric device through an external circuit to perform a photoelectric performance test.
[0072] Figure 6 The IV graphs of the photoelectric devices obtained in Example 1 and Example 2 under different excitation wavelength light sources at fixed power (conventional photoelectric test, test in air) are compared. Figure 6As shown in Figure 6a, the IV curves of the pure CdS device under different wavelengths of light have no obvious change trend, indicating that the broadband response of the pure CdS device is poor. Comparing the IV curves of the CdS / Bi2S3 heterojunction device under different wavelengths of UV-NIR (405-1060nm), as shown in Figure 6a, Figure 6 As shown in Figure 6b, the heterojunction device has a low dark current due to its obvious broadband photoresponse and strong photosensitivity. The obvious rectification characteristics show that it has typical photovoltaic behavior, indicating that an internal electric field is formed at the CdS / Bi2S3 heterojunction interface.
[0073] Figure 7 It is an IT diagram obtained by periodically switching the light source of the photoelectric device obtained by comparing Example 1 and Example 2. It can be seen that in the light-on state, the current increases rapidly and remains stable. After the power is turned off, the current decreases rapidly again, with excellent stability. This is due to the construction of the CdS / Bi2S3 Z-type heterojunction, which effectively separates the carriers and the mesh vertical structure has a fast carrier transmission path. When CdS and Bi2S3 are in close contact, the rearrangement of the Fermi level occurs, causing the energy band at the interface to bend, generating a built-in electric field, and forming a heterojunction. Under illumination, the electrons in the valence bands of CdS and Bi2S3 are excited to transition to the conduction band, and the electrons in the conduction band of Bi2S3 with a higher Fermi level are driven by the internal electric field to transfer to the valence band of CdS, effectively realizing the spatial separation of carriers, while suppressing the recombination of CdS and Bi2S3 electrons and holes, not only increasing the photocurrent, but also reducing the size of the dark current. At the same time, it can be seen that the heterojunction structure has a significant improvement in the performance of the photoelectric device. In addition, the fast carrier migration path of the mesh structure not only improves the light absorption capacity, but also expands the light absorption wavelength range.
[0074] Figure 8 The figure is a graph comparing the photocurrent and light power intensity of the photoelectric devices obtained in Example 1 and Example 2 under a fixed excitation wavelength light source. It can be clearly found in the figure that the response current increases with the increase of light power intensity, and compared with pure CdS, the photocurrent of the CdS / Bi2S3 heterojunction device is more dependent on light intensity, indicating that CdS and Bi2S3 have lower trap states and better photoelectric conversion capabilities at the interface.
[0075] Fig. 9The figure compares the responsivity R and the detection rate D of the photoelectric devices obtained in Example 1 and Example 2 under different excitation wavelength light sources. The performance of the photodetector is usually evaluated by the responsivity (R) and the specific detection rate (D), which can quantitatively evaluate the efficiency of the device in converting optical signals into electrical signals and the ability to detect weak optical signals. At the same time, the figure also shows the R and D of CdS and CdS / Bi2S3 heterojunction devices in the broadband range of 405-1060nm. The heterojunction device has obvious broadband response and performance improvement.
[0076] Fig.10 The IT diagrams of the optoelectronic device obtained in Example 1 at different powers under 405nm, 520nm, and 1060nm excitation wavelength light sources are shown in Figure 1. From the figure, it can be seen that the CdS / Bi2S3 heterojunction device has stable and excellent optoelectronic performance under different wavelengths of UV-NIR (405-1060nm).
[0077] Example 3 (for comparison)
[0078] A nanorod array-nanowire mesh heterojunction structure material grown on a FTO substrate, the preparation method being:
[0079] 1) Weigh 0.9mmol of thiourea, 0.18mmol of glutathione and 0.3mmol of cadmium nitrate tetrahydrate respectively and put them into a polytetrafluoroethylene liner, add 30mL of deionized water, and ultrasonicate to obtain a mixed solution. Put the washed and dried FTO glass with the conductive surface facing down, install a stainless steel autoclave, heat it to 200℃, and react for 4h under high temperature, high pressure and surfactant. After the reaction is completed, take out the FTO glass sample, rinse it with deionized water and ethanol, and obtain a glass sample of CdS nanorod array grown on FTO substrate.
[0080] 2) Then weigh 0.9mmol bismuth nitrate pentahydrate and 0.9mmol thiourea, put them into a polytetrafluoroethylene liner, add 30mL ethylene glycol, and ultrasonically obtain a mixed solution. The FTO glass sample prepared in step 1) is placed face down, and the stainless steel autoclave is installed, heated to 60°C, and reacted for 24h. After the reaction is completed, the FTO glass sample is taken out and rinsed with deionized water and ethanol to obtain a glass sample with a nanorod array-nanowire network heterojunction structure grown on an FTO substrate.
[0081] The application of the nanorod array-nanowire network heterojunction structure material grown on the FTO substrate prepared in Example 3 in a photodetector is specifically as follows:
[0082] The back of the glass sample was glued to the PCB board containing copper foil with silver paste, and then the conductive silver paste was dripped on the graphene surface and FTO substrate respectively, and high-purity silver wire was used as an external circuit connection. In this way, a simple device model of the photodetector can be made.
[0083] Example 4 (for comparison)
[0084] A nanorod array-nanowire mesh heterojunction structure material grown on a FTO substrate, the preparation method being:
[0085] 1) Weigh 0.9mmol of thiourea, 0.18mmol of glutathione and 0.3mmol of cadmium nitrate tetrahydrate respectively and put them into a polytetrafluoroethylene liner, add 30mL of deionized water, and ultrasonicate to obtain a mixed solution. Put the washed and dried FTO glass with the conductive surface facing down, install a stainless steel autoclave, heat it to 200℃, and react for 4h under high temperature, high pressure and surfactant. After the reaction is completed, take out the FTO glass sample, rinse it with deionized water and ethanol, and obtain a glass sample of CdS nanorod array grown on FTO substrate.
[0086] 2) Then weigh 0.1mmol bismuth nitrate pentahydrate and 0.1mmol thiourea, put them into a polytetrafluoroethylene liner, add 30mL ethylene glycol, and ultrasonically obtain a mixed solution. The FTO glass sample prepared in step 1) is placed face down, and the stainless steel autoclave is installed, heated to 60°C, and reacted for 24h. After the reaction is completed, the FTO glass sample is taken out and rinsed with deionized water and ethanol to obtain a glass sample with a nanorod array-nanowire mesh heterojunction structure grown on an FTO substrate.
[0087] The application of the nanorod array-nanowire network heterojunction structure material grown on the FTO substrate prepared in Example 4 in a photodetector is specifically as follows:
[0088] The back of the glass sample was glued to the PCB board containing copper foil with silver paste, and then the conductive silver paste was dripped on the graphene surface and FTO substrate respectively, and high-purity silver wire was used as an external circuit connection. In this way, a simple device model of the photodetector can be made.
[0089] Fig.11 This is a scanning electron microscope image of the CdS-Bi2S3 nanorod array-nanowire network heterojunction structure obtained in Example 3. It can be seen that the Bi2S3 content is too high, the crystal nuclei are agglomerated, and the growth is flake-like. The product with excessive Bi2S3 load has a flake-like morphology and is slightly poorly combined with the CdS nanorod array.
[0090] Fig.12The IT diagrams of the photoelectric device obtained in Example 3 under the excitation wavelengths of 405nm, 520nm, 650nm, 808nm and 1060nm are shown. It also has a broadband response, but compared with Example 1, the dark current is larger and the stability is slightly worse.
[0091] Fig.13 This is a scanning electron microscope image of the CdS-Bi2S3 nanorod array-nanowire network heterojunction structure obtained in Example 4. The loaded Bi2S3 content is too low, and the content of the network heterojunction structure after loading is too low. Although the network heterojunction structure remains unchanged after loading a small amount of Bi2S3, the loaded amount is obviously less.
[0092] Fig.14 The IT graphs of the photoelectric device obtained in Example 4 under a light source with an excitation wavelength of 520 nm are shown. Compared with Example 1, the dark current and stability are similar, the photocurrent is lower, and the improvement of the photoelectric performance is not obvious enough.
[0093] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a nanorod array-nanowire network heterojunction structure material grown on a FTO substrate, characterized in that: The preparation method comprises the following steps: 1) placing the FTO glass in an autoclave containing a sulfur source, a cadmium source, a surfactant and water, heating the autoclave to react, and obtaining a CdS nanorod array material grown on the FTO substrate; 2) The CdS nanorod array material grown on the FTO substrate prepared in step 1) is placed in an autoclave containing a sulfur source, a bismuth source and ethylene glycol, and heated to react to obtain a CdS-Bi2S3 nanorod array-nanowire network heterojunction structure material grown on the FTO substrate.
2. The preparation method according to claim 1, characterized in that: In step 1), the molar ratio of the sulfur source, the cadmium source and the surfactant is 0.3-0.9:0.1-0.3:0.06-0.
2.
3. The preparation method according to claim 1 or 2, characterized in that: In step 1), the surfactant is glutathione.
4. The preparation method according to claim 1 or 2, characterized in that: In step 1), the heating reaction refers to: reacting at 180-200° C. for 2-4 hours.
5. The preparation method according to claim 1, characterized in that: In step 2), the molar ratio of the sulfur source to the bismuth source is 0.3-0.6:0.2-0.
4.
6. The preparation method according to claim 1 or 5, characterized in that: The molar ratio of the cadmium source in step 1) to the bismuth source in step 2) is 0.1-0.3:0.2-0.
4.
7. The preparation method according to claim 1 or 5, characterized in that: In step 2), the heating reaction refers to: reacting at 60-80° C. for 18-24 hours.
8. A nanorod array-nanowire network heterojunction structure material grown on a FTO substrate prepared by the preparation method according to any one of claims 1 to 7.
9. An application of the nanorod array-nanowire network heterojunction structure material grown on the FTO substrate according to claim 8, characterized in that: Used for photoelectric detection.