Composite negative electrode material and preparation method and application thereof

By growing nano Si/SiOx in situ on biomass porous hard carbon to form Si/SiOx/C composite materials, the problems of insufficient conductivity and volume changes of silicon materials in lithium-ion batteries are solved, and the performance and life of the battery are improved. At the same time, it reduces production costs.

CN119050289APending Publication Date: 2024-11-29GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411023387.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The low conductivity of silicon materials in lithium-ion batteries and volume changes during charging and discharging lead to problems with electron transmission efficiency and structural stability, limiting their large-scale application.

Method used

Using silicon-rich biomass porous hard carbon as a support, nano Si/SiOx is grown in situ on it by chemical vapor deposition to form Si/SiOx/C composite material. Combined with high temperature carbonization and impurity removal treatment, a high ratio was prepared. Composite negative electrode material with surface area and excellent conductivity.

Benefits of technology

It improves the charging and discharging efficiency and power density of lithium-ion batteries, reduces the impact of volume expansion on the structure, extends the service life of the battery, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050289A_ABST
    Figure CN119050289A_ABST
Patent Text Reader

Abstract

The invention discloses a composite negative electrode material and a preparation method and application thereof. The silicon-carbon composite material Si / SiOx / C (x is more than 0 and less than 2) is prepared by taking a silicon-containing biomass crude product as a raw material and carrying out pre-carbonization, nano silicon in-situ growth, high-temperature carbonization and impurity removal treatment. In the high-temperature carbonization process, the overall expansion rate of the material is remarkably reduced through the neutralization reaction of silicon and silicon dioxide, so that the cycling stability of the electrode material is greatly improved. According to the method, the adopted biomass raw materials are wide in source and low in price, the preparation method is simple, energy-saving and high in operability, and a feasible solution is provided for application of large-scale energy storage batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a composite negative electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion secondary batteries have attracted much attention for their excellent energy density, long cycle life, and outstanding safety and reliability. This type of battery is not only widely used in various portable electronic devices, but has also gradually penetrated into key areas such as electric vehicles and large-scale energy storage systems. Among the negative electrode materials of lithium-ion batteries, silicon materials have excellent theoretical specific capacity (up to 3579mAh g -1 ), far exceeding the theoretical specific capacity of traditional graphite materials (only 372mAh g -1 ), and has therefore become a hot research focus in the field of scientific research at home and abroad. However, despite its huge potential, silicon materials still face two core challenges in large-scale application: one is its low conductivity, which limits the efficiency of electron transmission in silicon materials in batteries; the other is the severe volume change during the charging and discharging process, which may lead to damage to the battery structure and performance degradation.

[0003] In order to overcome these technical bottlenecks, the solutions currently adopted by researchers are mainly:

[0004] (1) Improving the structure of silicon-carbon composite materials, such as the Chinese invention patent application with publication number CN116477600A, reduces the physical strain and the critical fracture size of silicon particles by preparing a core-shell structure. A conductive bridge is formed between the amorphous carbon layer on the surface of the nano-silicon particles and the carbon network matrix material, which can not only effectively improve the conductivity of the nano-silicon particles, but also serve as a protective layer to buffer the volume expansion of the nano-silicon particles to maintain the overall stability of the material structure.

[0005] (2) Composite nano-silicon with other conductive materials, such as the Chinese invention patent application with publication number CN111009648A, which uses metal powder to reduce biomass-derived silicon dioxide at low temperature to prepare a silicon-carbon composite material in a one-step process. The prepared silicon-carbon composite material has a large specific surface area and high structural stability. When used as a negative electrode material for lithium-ion batteries, it exhibits high specific capacity and excellent cycle performance.

[0006] Although the above measures have alleviated the volume expansion and insufficient conductivity of silicon as anode materials to a certain extent, in actual industrial production, these measures still face multiple challenges such as high raw material costs, cumbersome and complex preparation processes, and easy introduction of impurities during the preparation process, which limits the large-scale application of silicon anode materials. Therefore, further research and exploration of more economical, efficient and pure preparation technologies are needed to promote the widespread application of silicon anode materials in the field of lithium-ion batteries. Summary of the invention

[0007] The main purpose of the present invention is to provide a composite negative electrode material and a preparation method and application thereof, which can improve the conductivity of silicon materials and the problem of volume expansion during charging and discharging and solve the problem of poor conductivity of silicon.

[0008] To achieve the above purpose, the technical solution of the present invention is as follows:

[0009] In a first aspect, the present invention provides a composite negative electrode material having a general formula of Si / SiO x / C, wherein 0<x<2; the composite negative electrode material uses silicon-rich biomass porous hard carbon as a carrier, and the nano-Si / SiO x In situ growth on biomass porous hard charcoal.

[0010] In at least one embodiment, the D50 of the biomass porous hard carbon is 15-25 μm, and the specific surface area is 5-10 m 2 ·g -1 , the porosity is 5% to 20%, and the atomic percentage of silicon is 10% to 30%; the atomic percentage of silicon in the composite negative electrode material is 20% to 40%, the atomic percentage of carbon is 60% to 80%, and SiO x It accounts for 30% to 40% of the composite material.

[0011] In a second aspect, the present invention further provides a method for preparing a composite negative electrode material, comprising the following steps:

[0012] 1) Pre-carbonizing the silicon-rich biomass crude product at 400° C. to 600° C. to obtain biomass porous hard carbon;

[0013] 2) In-situ growth of nano-silicon on pre-carbonized biomass porous hard carbon to obtain a composite material precursor;

[0014] 3) carbonizing the composite material precursor at a temperature of 900° C. to 1350° C., and cooling the composite material to obtain the composite material;

[0015] 4) The composite material is subjected to impurity removal, crushing and screening treatment to obtain the composite negative electrode material.

[0016] In a third aspect, the present invention also provides the use of the aforementioned composite negative electrode material in preparing a lithium battery or a lithium ion supercapacitor. Specifically, the lithium battery can be an organic solvent lithium ion battery, an aqueous lithium ion battery, a semi-solid lithium battery or an all-solid lithium battery.

[0017] Compared with the prior art, the present invention can at least achieve the following technical effects:

[0018] 1. The present invention provides a composite negative electrode material, the general formula of which is Si / SiO x / C(0<x<2),Si / SiO x / C(0<x<2) uses silicon-containing biomass porous hard carbon as a carrier, nano-Si / SiO x In situ growth on biomass porous hard carbon. Silicon materials will undergo severe volume expansion and contraction during the charge and discharge process, which will lead to structural damage and performance degradation of electrode materials. x In-situ growth on biomass porous hard carbon can effectively alleviate this volume expansion, because the pore structure of biomass porous hard carbon can accommodate the volume change of silicon material, thereby maintaining the stability of nano-silicon / biomass hard carbon composite materials. Nano-silicon has a small particle size and a large specific surface area, which can provide more reactive sites. At the same time, biomass porous hard carbon has good conductivity, which is conducive to the transmission of electrons. Therefore, in-situ growth of nano-silicon on biomass hard carbon can improve the electronic and ion transmission properties of the composite material, thereby improving the charge and discharge efficiency and power density of lithium-ion batteries. Biomass porous hard carbon comes from renewable biomass resources and has the advantages of environmental protection and sustainability. The use of composite negative electrode materials can not only improve the performance of lithium-ion batteries, but also reduce production costs.

[0019] 2. The present invention also provides a method for preparing a composite negative electrode material, using silicon-rich crude bagasse and nano-silicon as raw materials. The early pre-carbonization increases the porous structure of the precursor material and improves the pore structure, so that the silicon dioxide in the biomass waste is more exposed, which is beneficial to the subsequent neutralization reaction, reduces the side reactions such as the generation of lithium silicate by the negative electrode of the battery during the charging and discharging process, reduces the loss of lithium ions, and increases the service life of the battery. The present invention performs carbonization at 900-1350°C, which can effectively avoid the occurrence of side reactions (such as the reaction of Si and C at high temperature to generate SiC), making the purity of the silicon-carbon composite material higher. The porous Si / SiO prepared by the present invention x The nano-silicon / biomass hard carbon composite material prepared by the present invention is used in lithium-ion batteries, and the battery's first charge specific capacity can reach 1000mAh·g -1 The above is much higher than the specific capacity of the existing biomass porous hard carbon as anode (188 mAh g -1 ), which can be used as the negative electrode of high energy density lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] One or more embodiments of the present application will now be described, by way of example only, with reference to the accompanying drawings, in which:

[0021] Figure 1 XRD diagram of the composite negative electrode material provided in Example 1;

[0022] Figure 2 A cycle performance diagram of the composite negative electrode material provided in Example 1;

[0023] Figure 3 A charge and discharge curve diagram of the composite negative electrode material provided in Example 1;

[0024] Figure 4 This is the charge and discharge curve diagram of the biomass porous hard carbon negative electrode material provided in Comparative Example 1. DETAILED DESCRIPTION

[0025] It will be understood that the terms or words used in the specification and claims of the present invention should not be interpreted as limited to the meanings defined in common dictionaries. It will be further understood that, based on the principle that the inventor can appropriately define the meanings of terms or words to best explain the present invention, these terms or words should be interpreted as having a meaning consistent with the meaning in the context of the technical concept of the present invention and the related technology.

[0026] The terminology used herein is for the purpose of describing particular exemplary embodiments only and is not intended to be limiting of the present invention. Terms in the singular may include plural forms unless the context clearly indicates otherwise.

[0027] It will be further understood that when used in this specification, the terms "comprises", "comprising" or "having" specify the presence of stated features, numbers, steps, elements or combinations thereof, but do not exclude the presence or addition of one or more other features, numbers, steps, elements or combinations thereof.

[0028] In the present specification, "%" means weight % (wt %) unless otherwise specified.

[0029] In this specification, the "specific surface area" is measured by the BET method, and specifically, can be calculated from the adsorption amount of nitrogen at liquid nitrogen temperature (77K) using Belsorp-mini II of BEL Japan Co., Ltd.

[0030] In this specification, "porosity" refers to the proportion of voids in the positive and negative electrode materials of the battery. The methods for determining porosity include the following: mercury intrusion method, density method, BET method (gas adsorption method), imbibition method, and statistical method. Among them, mercury intrusion method and BET method are the more commonly used methods in daily laboratories.

[0031] In this specification, the average particle size (D50) may be defined as the particle size corresponding to 50% of the volume accumulation in the particle size distribution curve of the particles. The average particle size (D50) may be measured, for example, by a laser diffraction method. The laser diffraction method is generally capable of measuring particle sizes ranging from the submicron range to several millimeters, thereby obtaining results with high reproducibility and high resolution.

[0032] In this specification, chemical vapor deposition (CVD) is a typical bottom-up method for preparing ultra-thin two-dimensional nanomaterials. In the preparation process of this method, a given substrate is placed in a special gas environment, and a reaction occurs on the surface of the substrate to form an ultra-thin two-dimensional sheet or a large-area ultra-thin film, which can produce ultra-thin two-dimensional nanomaterials with high crystal quality, scalable size, and adjustable thickness.

[0033] Hereinafter, the present invention will be described in more detail.

[0034] First, the present invention provides a composite negative electrode material, the general formula of which is Si / SiO x / C, wherein 0<x<2; the composite negative electrode material uses silicon-rich biomass porous hard carbon as a carrier, and the nano-Si / SiO x In situ growth on biomass porous hard charcoal.

[0035] Specifically, the SiO x It can be SiO, because it contains SiO x , thus the capacity of the battery can be increased.

[0036] Specifically, the D50 of the biomass porous hard carbon is 15-25 μm, and the specific surface area is 5-10 m2·g -1 , the porosity is 5% to 20%, and the atomic percentage of silicon is 10% to 30%; the atomic percentage of silicon in the composite negative electrode material is 20% to 40%, the atomic percentage of carbon is 60% to 80%, and SiO x It accounts for 30% to 40% of the composite material.

[0037] More specifically, the method for preparing the biomass porous hard carbon is to pre-carbonize the silicon-rich biomass crude product at 400° C. to 600° C. The in-situ growth adopts a chemical vapor deposition method.

[0038] The composite negative electrode material can be used in the preparation of lithium batteries or lithium ion supercapacitors, and is generally used to prepare the negative electrode of lithium batteries.

[0039] The negative electrode of the battery includes a negative electrode active material layer, and the negative electrode active material layer includes the above-mentioned composite negative electrode material. The negative electrode of the battery may also include a negative electrode collector supporting the negative electrode active material layer, and the negative electrode active material layer should be evenly coated on the surface of the negative electrode collector. The material used for the negative electrode collector is not limited, as long as it has conductivity and does not cause chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, or aluminum or stainless steel surface-treated with one of nickel, titanium, silver and the like can be used. Specifically, the prepared composite negative electrode material and carbon black can be evenly mixed, an appropriate amount of deionized water can be added to form a uniform slurry, which is applied on a copper foil and dried to obtain a negative electrode sheet.

[0040] The lithium battery can be an organic solvent lithium ion battery, an aqueous lithium ion battery, a semi-solid lithium battery or an all-solid lithium battery. Specifically, the structure of the battery may include a negative electrode, a positive electrode, a diaphragm inserted between the positive electrode and the negative electrode, and an electrolyte. More specifically, LiPF6 / EC-DEC-EMC can be used as an electrolyte, a metal lithium sheet as a counter electrode, and a Celgard2400 polypropylene film as a diaphragm, and the battery can be assembled in an argon-protected glove box.

[0041] Secondly, the present invention also provides a method for preparing a composite negative electrode material, the method comprising the following steps:

[0042] 1) Pre-carbonizing the silicon-rich biomass crude product at 400° C. to 600° C. to obtain biomass porous hard carbon;

[0043] 2) In-situ growth of nano-silicon on pre-carbonized biomass porous hard carbon to obtain a composite material precursor;

[0044] 3) carbonizing the composite material precursor at a temperature of 900° C. to 1350° C., and cooling the composite material to obtain the composite material;

[0045] 4) The composite material is subjected to impurity removal, crushing and screening treatment to obtain the composite negative electrode material.

[0046] Specifically, the crude biomass product is one or a combination of any of bagasse, corn stalks, macadamia nut shells, reed bamboo and eucalyptus. The silicon-rich degree or silicon-containing degree of the crude biomass product is such that the silicon atomic percentage of the porous hard carbon of the biomass reaches 10% to 30%.

[0047] Specifically, the molar ratio of the biomass porous hard carbon to the nano-silicon is 1-1.5:1, and the D50 of the nano-silicon is 2-150 nm.

[0048] Specifically, the high temperature carbonization time is 0.5h to 2h, and the high temperature carbonization is performed under an inert gas, which may be one of nitrogen, argon and ammonia, or any combination of multiple thereof.

[0049] Specifically, the impurity removal is performed by washing with an acidic solution and deionized water; generally, acid washing is performed first, and then water washing, which can be performed several times in turn until the water washing solution is neutral. Further, the concentration of the acidic solution is 0.5-5 mol / L, and the acidic solution can be at least one of a hydrochloric acid solution, a phosphoric acid solution, and a nitric acid solution. The pulverization can be one of air flow milling, ball milling, and sand milling, or any combination of multiple thereof.

[0050] Hereinafter, the present invention will be described by way of examples.

[0051] Example 1

[0052] A method for preparing a composite negative electrode material comprises the following steps:

[0053] (1) 0.75 g of crude silicon-containing bagasse was pre-carbonized at 400° C. to obtain a porous hard biocarbon; 0.5 g of nano-silicon with a D50 of 100 nm was in-situ grown on the porous biocarbon by chemical vapor deposition to obtain a porous hard biocarbon precursor;

[0054] (2) carbonizing the bagasse porous hard carbon precursor obtained in step (1) at 900° C. for 2 h under a nitrogen atmosphere, and cooling to obtain a composite material;

[0055] (3) The composite material obtained in step (2) is crushed and sieved by a jet mill, and washed repeatedly with a hydrochloric acid solution (with a concentration of 0.5 mol / L) and deionized water in turn until it is neutral, to obtain a composite negative electrode material with uniform particle size.

[0056] Figure 1 The XRD pattern of the composite negative electrode material prepared in Example 1 of the present invention is shown in FIG. Figure 1 It can be seen that the composite negative electrode material of the present invention has crystal structure peaks of silicon and carbon.

[0057] The composite negative electrode material and super carbon black prepared in Example 1 were mixed uniformly in a mass ratio of 90:10, and an appropriate amount of deionized water was added to form a uniform slurry, which was coated on a copper foil and vacuum dried at 80°C for 12 hours to obtain an electrode sheet. 1.0M LiPF6 / EC-DEC-EMC (volume ratio of 1:1:1) was used as the electrolyte, a metal lithium sheet was used as the counter electrode, and a Celgard2400 polypropylene film was used as the diaphragm. The battery was assembled in an argon-protected glove box. After the assembled battery was allowed to stand for 24 hours, a LAND electrochemical tester was used for performance testing. The voltage range of the charge and discharge test was 0.01-1.5V, and the current density was 50mA·g -1 .

[0058] Figure 2This is a cycle performance diagram of the composite negative electrode material prepared in Example 1 of the present invention. Figure 3 The charge and discharge curve of the composite negative electrode material prepared in Example 1 of the present invention is shown in Figure 1. It can be seen that the initial charge specific capacity of the composite negative electrode material is 1317 mAh·g -1 , the first coulombic efficiency is 87%.

[0059] Example 2

[0060] A method for preparing a composite negative electrode material comprises the following steps:

[0061] (1) 0.75 g of crude silicon-containing bagasse was pre-carbonized at 450° C. to obtain a porous hard biomass carbon; 0.67 g of nano-silicon with a D50 of 100 nm was in-situ grown on the porous biomass carbon by chemical vapor deposition to obtain a porous hard biocarbon precursor;

[0062] (2) carbonizing the bagasse porous hard carbon precursor obtained in step (1) at 1000° C. for 2 h under a nitrogen atmosphere, and cooling to obtain a composite material;

[0063] (3) The composite material obtained in step (2) is crushed and sieved by a jet mill, and washed repeatedly with a hydrochloric acid solution (with a concentration of 0.5 mol / L) and deionized water in turn until it is neutral, to obtain a composite negative electrode material with uniform particle size.

[0064] The battery was assembled according to the method of assembling the battery in Example 1, and the charge and discharge test was performed on it. At a current density of 50 mA·g -1 The first charge specific capacity of the composite negative electrode material of this embodiment is 1025 mAh g -1 , the first coulombic efficiency is 92%.

[0065] Example 3

[0066] A method for preparing a composite negative electrode material comprises the following steps:

[0067] (1) 0.75 g of silicon-containing reed bamboo crude product was pre-carbonized at 400° C. to obtain a biomass porous hard carbon; 0.5 g of nano-silicon with a D50 of 100 nm was in-situ grown on the biomass porous hard carbon by chemical vapor deposition to obtain a reed bamboo porous hard carbon precursor;

[0068] (2) carbonizing the porous hard carbon precursor of Phragmites australis obtained in step (1) at 900° C. for 2 h under a nitrogen atmosphere, and cooling to obtain a composite material;

[0069] (3) The composite material obtained in step (2) is crushed and sieved by a jet mill, and washed repeatedly with a hydrochloric acid solution (with a concentration of 0.5 mol / L) and deionized water in turn until it is neutral, to obtain a composite negative electrode material with uniform particle size.

[0070] The battery was assembled according to the method of assembling the battery in Example 1, and the charge and discharge test was performed on it. At a current density of 50 mA·g -1 The first charge specific capacity of the composite negative electrode material of this embodiment is 952 mAh g -1 , the first coulombic efficiency is 85%.

[0071] Example 4

[0072] A method for preparing a composite negative electrode material comprises the following steps:

[0073] (1) 0.75 g of crude silicon-containing eucalyptus was pre-carbonized at 400° C. to obtain a biomass porous hard carbon; 0.5 g of nano-silicon with a D50 of 100 nm was in-situ grown on the biomass porous hard carbon by chemical vapor deposition to obtain a eucalyptus porous hard carbon precursor;

[0074] (2) carbonizing the eucalyptus porous hard carbon precursor obtained in step (1) at 900° C. for 2 h under a nitrogen atmosphere, and cooling to obtain a composite material;

[0075] (3) The composite material obtained in step (2) is crushed and sieved by a jet mill, and washed repeatedly with a hydrochloric acid solution (with a concentration of 0.5 mol / L) and deionized water in turn until it is neutral, to obtain a composite negative electrode material with uniform particle size.

[0076] The battery was assembled according to the method of assembling the battery in Example 1, and the charge and discharge test was performed on it. At a current density of 50 mA·g -1 The first charge specific capacity of the composite negative electrode material of this embodiment is 905 mAh g -1 , the first coulombic efficiency is 89%.

[0077] Comparative Example 1

[0078] A method for preparing a biomass hard carbon negative electrode material, wherein the preparation method is substantially the same as the preparation method of Example 1 except that nano-silicon is not added, and the remaining steps include the following steps: (1) pre-carbonizing 0.75 g of crude silicon-containing bagasse at 400° C.; (2) carbonizing the obtained bagasse porous hard carbon composite material precursor at 900° C. for 2 h under a nitrogen atmosphere, and cooling to obtain a composite material; (3) crushing and sieving the obtained composite material with a jet mill, and repeatedly washing with a hydrochloric acid solution (with a concentration of 0.5 mol / L) and deionized water until neutral, to obtain a biomass hard carbon negative electrode material with uniform particle size.

[0079] The battery was assembled according to the method of assembling the battery in Example 1, and the charge and discharge test was performed on it. At a current density of 50 mA·g -1The first charge specific capacity of the biomass hard carbon negative electrode material of this embodiment is 188 mAh g -1 , the first coulombic efficiency is 71%.

[0080] The performance indicators of the lithium-ion batteries of the embodiments of the present invention and the comparative examples are shown in Table 1.

[0081] Table 1. Performance indicators of lithium-ion batteries

[0082] Examples <![CDATA[Reversible specific capacity (mAh·g -1 )]]> First coulombic efficiency Voltage range(V) Example 1 1317 87% 0.01-1.5 Example 2 1025 92% 0.01-1.5 Example 3 952 85% 0.01-1.5 Example 4 905 89% 0.01-1.5 Comparative Example 1 188 71% 0.01-1.5

[0083] It can be seen from Table 1 that, compared with the common biomass porous hard carbon negative electrode material (Comparative Example 1), the nano-silicon / porous biomass hard carbon composite negative electrode material of the present invention has a higher first charge specific capacity.

[0084] At the same time, compared with Example 2, the first coulombic efficiency of the carbon composite negative electrode material obtained in Example 1 is higher, because: the chemical properties of silicon and carbon in the silicon-carbon composite material are complementary. Nano silicon has excellent high temperature resistance and chemical stability, while porous biomass hard carbon has excellent electrical conductivity and thermal conductivity. By reducing the mass of silicon, the proportion of carbon in the composite material is relatively increased, which helps to optimize the electrochemical properties of the composite material, such as improving conductivity and reducing resistance, thereby improving the first coulombic efficiency.

[0085] In addition, compared with Examples 3 and 4, the composite negative electrode materials prepared in Examples 1 and 2 have a higher first charge specific capacity, because: the bagasse porous hard carbon negative electrode material has a richer pore structure than other biomass-derived porous hard carbons, which is conducive to the infiltration of electrolytes and the rapid diffusion of ions, thereby improving the charging capacity of lithium-ion batteries. Furthermore, the high-temperature carbonization product of bagasse has a three-dimensional skeleton and a large specific surface area. This multi-level pore structure effectively provides an electron transmission channel, which is manifested as a high first charge specific capacity of lithium-ion batteries.

[0086] In summary, the present invention prepares a composite negative electrode material by the reaction of high temperature carbonized silicon and silicon dioxide, and its general formula is Si / SiO x / C(0<x<2). The preparation method of the present invention combines the advantages of nano-silicon and porous biomass hard carbon, and undergoes the technology of "pre-carbonization, in-situ growth of nano-silicon, high-temperature carbonization and impurity removal". A new type of composite negative electrode material is prepared, which has the advantages of high specific capacity, high first coulomb efficiency, excellent cycle performance, etc., improves the electron transmission efficiency of silicon materials in batteries and reduces the problem of volume expansion of nano-silicon during charging and discharging.

[0087] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A composite negative electrode material, characterized in that: The general formula of the composite negative electrode material is Si / SiO x / C, wherein 0<x<2; the composite negative electrode material uses silicon-rich biomass porous hard carbon as a carrier, and the nano-Si / SiO x In situ growth on biomass porous hard charcoal.

2. The composite negative electrode material according to claim 1, characterized in that The biomass porous hard carbon has a D50 of 15 to 25 μm and a specific surface area of ​​5 to 10 m 2 ·g -1 , the porosity is 5% to 20%, and the atomic percentage of silicon is 10% to 30%; the atomic percentage of silicon in the composite negative electrode material is 20% to 40%, the atomic percentage of carbon is 60% to 80%, and SiO x It accounts for 30% to 40% of the composite material.

3. The composite negative electrode material according to claim 1, characterized in that The method for preparing the biomass porous hard carbon is to perform a pre-carbonization treatment on a silicon-rich biomass crude product at 400°C to 600°C.

4. The composite negative electrode material according to claim 1, characterized in that The in-situ growth adopts a chemical vapor deposition method.

5. A method for preparing a composite negative electrode material, characterized in that: The steps include: 1) Pre-carbonizing the silicon-rich biomass crude product at 400° C. to 600° C. to obtain biomass porous hard carbon; 2) In-situ growth of nano-silicon on pre-carbonized biomass porous hard carbon to obtain a composite material precursor; 3) carbonizing the composite material precursor at a temperature of 900° C. to 1350° C., and cooling the composite material to obtain the composite material; 4) The composite material is subjected to impurity removal, crushing and screening treatment to obtain the composite negative electrode material.

6. The preparation method according to claim 5, characterized in that: The crude biomass product is one or a combination of any multiple of bagasse, corn stalks, macadamia nut shells, reed bamboo and eucalyptus.

7. The preparation method according to claim 5, characterized in that: The molar ratio of the biomass porous hard carbon to the nano silicon is 1-1.5:1, and the D50 of the nano silicon is 2-150nm.

8. The preparation method according to claim 5, characterized in that: The high temperature carbonization time is 0.5h to 2h, and the high temperature carbonization is carried out under an inert gas.

9. The preparation method according to claim 5, characterized in that: The impurity removal is performed by washing with an acidic solution and deionized water.

10. Use of the composite negative electrode material according to any one of claims 1 to 4 or the composite negative electrode material prepared by the preparation method according to any one of claims 5 to 9 in the preparation of lithium batteries or lithium ion supercapacitors.