Manufacturing method of phase change memory
By using a thin silicon-containing antireflection layer as the etching mask of the carbon mask layer in phase change memory manufacturing, the thickness of the SiO2 layer and the thickness of the PR layer are reduced, and the problems of high cost and slow speed in the prior art are solved. , achieving low cost and rapid manufacturing.
Patent Information
- Application Number
- CN202411052916.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-29
AI Technical Summary
In the existing phase change memory manufacturing methods, the SiO2 layer has high thickness requirements and is prone to erosion, resulting in high cost and slow manufacturing speed, requiring a large amount of PR material and time.
The thickness of the silicon-containing anti-reflective layer (SHB layer) is less than 80 nanometers as an etching mask for the carbon mask layer, which reduces the thickness requirement of the SiO2 layer, and the SHB layer is etched by the patterned photoresist layer to form Patterned carbon mask layer reduces the thickness and usage of the PR layer.
Reduces manufacturing costs, improves manufacturing speed, and reduces PR material usage and coating time.
Smart Images

Figure CN119053157A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor integrated circuit manufacturing, and in particular to a method for manufacturing a phase change memory. Background Art
[0002] In the manufacture of semiconductor integrated circuits, especially in the manufacture of phase change memory, the requirements for photolithography technology are becoming increasingly higher. Figure 8 As shown, in the prior art phase change memory manufacturing, in order to form a desired pattern on the GST (phase change material) layer 91, a TiN (titanium nitride) layer 92, a SiN (silicon nitride) layer 93, a carbon HM (mask) layer 94, a SiO2 (silicon dioxide) layer 97, an ARC layer (anti-reflective layer) 95, and a PR (photoresist) layer 96 are usually formed in sequence on the GST layer 91 to form a laminate 900. Then, the PR layer 96 is photolithographically processed to form a patterned PR layer. Then, the ARC layer 95, the SiO2 layer 97, the carbon HM layer 94, the SiN layer 93, the TiN layer 92, and the GST layer 91 are etched in sequence through the patterned PR layer to form a patterned GST layer.
[0003] Among them, the function of the ARC layer 95 is to absorb reflected light in the photolithography process and improve the photolithography accuracy. The function of the SiO2 layer 97 is to serve as a mask in the etching process of the carbon HM layer 94. Because the PR layer 96 and the ARC layer 95 are both relatively soft and cannot serve as masks in the etching process of the carbon HM layer 94, a layer of SiO2 layer 97 must be formed under the ARC layer 95, and the carbon HM layer 94 is etched using the SiO2 layer 97 as a mask. In addition, the thickness of the SiO2 layer 97 must be relatively thick, usually above 80 nanometers. Because when the carbon HM layer 94 is etched, the SiO2 layer 97 will also be eroded and gradually become thinner. If the thickness of the SiO2 layer 97 is not enough, the SiO2 layer 97 will be completely eroded before the carbon HM layer 94 is completely patterned, so it cannot serve as a mask. In addition, because the thickness of the SiO2 layer 97 is relatively large, a relatively thick PR layer 96 is also required to be used as a mask when etching the SiO2 layer 97. Usually, the thickness of the PR layer 96 is greater than 300 nanometers. Therefore, it is necessary to apply more PR material, which increases the cost. In addition, the time required for applying PR is also relatively long, thereby reducing the manufacturing speed.
[0004] Therefore, the industry is in urgent need of a low-cost and high-speed manufacturing method for phase change memory. Summary of the invention
[0005] The present invention aims to provide a method for manufacturing a phase change memory with low cost and high speed.
[0006] The manufacturing method of the phase change memory of the present invention comprises:
[0007] a laminate forming step, forming a laminate on a semiconductor substrate, the laminate comprising a phase change material layer, a titanium nitride layer, a silicon nitride layer, a carbon mask layer, a silicon-containing anti-reflection layer, and a photoresist layer sequentially formed from bottom to top, wherein the thickness of the silicon-containing anti-reflection layer is less than 80 nanometers;
[0008] A photolithography step of exposing and developing the photoresist layer to form a patterned photoresist layer;
[0009] A first etching step, etching the silicon-containing anti-reflection layer through the patterned photoresist layer to form a patterned silicon-containing anti-reflection layer;
[0010] a second etching step of etching the carbon mask layer through the patterned silicon-containing anti-reflection layer to form a patterned carbon mask layer;
[0011] a third etching step of etching the silicon nitride layer through the patterned carbon mask layer to form a patterned silicon nitride layer; and
[0012] In a fourth etching step, the titanium nitride layer and the phase-change material layer are etched through the patterned silicon nitride layer to form a patterned titanium nitride layer and a patterned phase-change material layer.
[0013] The manufacturing method of the phase change memory of the present invention can reduce the manufacturing cost and improve the manufacturing speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is a flow chart of a method for manufacturing a phase change memory of the present invention;
[0015] Figures 2 to 7 is a schematic diagram of various steps of forming a patterned GST layer of the present invention; and
[0016] Figure 8 It is a schematic diagram of a laminated body of a method for manufacturing a phase change memory in the prior art.
[0017] Explanation of symbols
[0018] 100,900 laminated body
[0019] 1,91GST layer
[0020] 2. 92TiN layer
[0021] 3.93SiN layer
[0022] 4, 94 carbon HM layer
[0023] 5SHB layer
[0024] 6, 96PR layer
[0025] 11Patterned GST layer
[0026] 12 Patterned TiN layer
[0027] 13 Patterning SiN layer
[0028] 14 Patterned Carbon HM Layer
[0029] 15 Patterned SHB layer
[0030] 16 Patterned PR layer
[0031] 95ARC layer
[0032] 97SiO2 layer DETAILED DESCRIPTION
[0033] Refer to the following Figures 1 to 7 The manufacturing method of the phase change memory of the present invention is described. Figure 1 As shown, the manufacturing method of the phase change memory of the present invention includes: a stacked body forming step S001, a photolithography step S002, a first etching step S003, a second etching step S004, a third etching step S005, and a fourth etching step S006. Each step will be described in detail below in conjunction with the accompanying drawings.
[0034] The layered body forming step S001, Figure 2 As shown, a laminate 100 is formed on a semiconductor substrate (not shown), and the laminate 100 includes a GST layer 1, a TiN layer 2, a SiN layer 3, a carbon HM layer 4, an SHB layer (Si rich hard mask bottom ARC, silicon-containing anti-reflection layer) 5, and a PR layer 6, which are formed in sequence from bottom to top, wherein the thickness of the SHB layer 5 is less than 80 nanometers.
[0035] In this embodiment, a GST layer 1 and a TiN layer 2 are first formed on a semiconductor substrate by a PVD (physical vapor deposition) process. The GST layer 1 and the TiN layer 2 may be formed directly on the semiconductor substrate, or there may be other layers between the semiconductor substrate and the GST layer 1 and the TiN layer 2. Then, a SiN layer 3 is formed on the TiN layer 2 by a CVD process. The SiN layer 3 may be formed directly on the TiN layer 2, or there may be other layers between the TiN layer 2 and the SiN layer 3. Then, a carbon HM layer 4, an SHB layer 5, and a PR layer 6 are sequentially formed on the SiN layer 3 by a coating process.
[0036] Due to the properties of the GST layer 1 and the TiN layer 2, SiN needs to be used as a mask for etching. Therefore, it is necessary to first form a SiN layer 3 on the GST layer 1 and the TiN layer 2. Before etching the GST layer 1 and the TiN layer 2, the SiN layer 3 must be etched first to form a patterned SiN layer, and then the GST layer 1 and the TiN layer 2 are etched through the patterned SiN layer. Because the SiN layer 3 is relatively hard and difficult to etch, when etching the SiN layer 3, the PR layer 6 and the SHB layer 5 cannot be directly used as a mask for the SiN layer 3. A carbon HM layer 4 must be formed on the SiN layer 3, and the carbon HM layer 4 must be used as a mask for the SiN layer 3 for etching.
[0037] Among them, the SHB layer 5 can play an anti-reflective role, so that it can absorb reflected light in the photolithography process and improve the photolithography accuracy, so that the ARC layer is not needed. In addition, because the SHB layer 5 contains silicon, its hardness is relatively large, so it can be used as a mask for etching the carbon HM layer 4. In this way, there is no need to form a SiO2 layer on the carbon HM layer 4. In addition, when the carbon HM layer 4 is etched, the SHB layer 5 is less corroded, so the SHB layer 5 can be made relatively thin, which can be less than 80 nanometers, or even less than 70 nanometers. According to experimental results, when the thickness of the SHB layer 5 is 70 nanometers, when the carbon HM layer 4 is etched, when the carbon HM layer 4 is completely patterned, the SHB layer 5 is still not completely corroded.
[0038] Preferably, the thickness of the PR layer 6 is less than 300 nanometers. Because the thickness of the SHB layer 5 is reduced, when etching the SHB layer 5, a PR layer 6 that is too thick is not needed as a mask. In this embodiment, the thickness of the PR layer 6 may be less than 300 nanometers. In other embodiments, the thickness of the PR layer 6 may be less than 270 nanometers. According to experimental results, when the thickness of the PR layer 6 is 270 nanometers, when etching the SHB layer 5, when the SHB layer 5 is completely patterned, the PR layer 6 is still not completely eroded.
[0039] Because the thickness of the PR layer 6 is reduced, the PR material used is reduced, thus reducing the cost. In addition, because the thickness of the PR layer 6 is reduced, the time for coating PR is reduced, and the time for coating PR on each wafer is reduced, which can speed up the entire manufacturing process.
[0040] Photolithography step S002, such as Figure 3 As shown, the PR layer 6 is exposed and developed to form a patterned PR layer 16. The PR layer 6 can be exposed and developed in any suitable manner in the prior art, which will not be described in detail herein.
[0041] The first etching step S003, such as Figure 4As shown, the SHB layer 5 is etched through the patterned PR layer 16 to form a patterned SHB layer 15 .
[0042] The second etching step S004, such as Figure 5 As shown, the carbon HM layer 4 is etched through the patterned SHB layer 15 to form a patterned carbon HM layer 14 .
[0043] The third etching step S005, such as Figure 6 As shown, the SiN layer 3 is etched through the patterned carbon HM layer 14 to form a patterned SiN layer 13 .
[0044] The fourth etching step S006, such as Figure 7 As shown, the TiN layer 2 and the GST layer 1 are etched through the patterned SiN layer 13 to form the patterned TiN layer 12 and the patterned GST layer 11. In addition, after the patterned TiN layer 12 and the patterned GST layer 11 are formed, a thin layer of SiN will remain on the top of the patterned TiN layer 12, and this layer of SiN can be used as a protective layer and an insulating layer for the patterned TiN layer 12 and the patterned GST layer 11 in subsequent processes.
[0045] The SHB layer 5 , the carbon HM layer 4 , the SiN layer 3 , the TiN layer 2 and the GST layer 1 may be etched in any suitable manner in the prior art, which will not be described in detail herein.
[0046] The phase change memory manufacturing method of the present invention can reduce manufacturing costs and increase manufacturing speed.
[0047] Although the present invention has been disclosed in the above embodiments, it is not intended to limit the present invention. Any professional and technical personnel in the field may make various necessary changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined by the attached claims.
Claims
1. A method for manufacturing a phase change memory, comprising: A laminate forming step S001, forming a laminate (100) on a semiconductor substrate, wherein the laminate (100) comprises a phase change material layer (1), a titanium nitride layer (2), a silicon nitride layer (3), a carbon mask layer (4), a silicon-containing anti-reflection layer (5), and a photoresist layer (6) formed in sequence from bottom to top, wherein the thickness of the silicon-containing anti-reflection layer (5) is less than 80 nanometers; Photolithography step S002, exposing and developing the photoresist layer (6) to form a patterned photoresist layer (16); A first etching step S003, etching the silicon-containing anti-reflection layer (5) through the patterned photoresist layer (16) to form a patterned silicon-containing anti-reflection layer (15); A second etching step S004, etching the carbon mask layer (4) through the patterned silicon-containing anti-reflection layer (15) to form a patterned carbon mask layer (14); A third etching step S005, etching the silicon nitride layer (3) through the patterned carbon mask layer (14) to form a patterned silicon nitride layer (13); and In a fourth etching step S006, the titanium nitride layer (2) and the phase change material layer (1) are etched through the patterned silicon nitride layer (13) to form a patterned titanium nitride layer (12) and a patterned phase change material layer (11).
2. The method for manufacturing a phase change memory according to claim 1, characterized in that: The thickness of the photoresist layer (6) is less than 300 nanometers.