Thermoelectric material based on N-type polycrystalline SnSe and preparation method thereof

By introducing In3+ and Br- into N-type polycrystalline SnSe thermoelectric material, InBr3 doped materials are prepared, which solves the problems of low electrical transmission performance and difficulty in synergistically improving electrical and thermal performance, and achieves high electrical transmission and low thermal transmission performance Coordinated optimization, the maximum power factor and thermoelectric superiority have been significantly improved.

CN119053225AInactive Publication Date: 2024-11-29SUN YAT SEN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411147635.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The N-type polycrystalline SnSe-based thermoelectric materials have low electrical transmission performance and are difficult to coordinately improve the electrical and thermal performance, which limits their application range.

Method used

By introducing high-priced cation In3+ and low-priced anion Br-, InBr3-doped SnSe material is prepared, which optimizes the electrical and heat transfer performance of the material. The specific steps include selecting the appropriate raw material molar ratio and high-purity raw material for melting reaction, and controlling the reaction conditions to achieve synergistic optimization of electrical and thermal conductivity.

Benefits of technology

The coordinated optimization of the electrical transmission and thermal transmission performance of N-type polycrystalline SnSe thermoelectric materials is achieved, so that the maximum power factor reaches 502μW m-1·K-2 and the thermoelectric superior value ZT reaches 1.4, solving the problem of low electrical performance and difficulty in synergistic improvement. Electrical and thermal performance issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053225A_ABST
    Figure CN119053225A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thermoelectric materials, and particularly relates to an N-type polycrystalline SnSe-based thermoelectric material and a preparation method thereof. The N-type polycrystalline SnSe thermoelectric material disclosed by the invention is an InBr3-doped SnSe material, the molar ratio of Sn to Se to InBr3 is (1-x): (0.93-3x): x, and x is more than 0 and less than or equal to 0.0075. By introducing a high-valence cation In < 3 + > and a low-valence anion Br <->, the carrier concentration is improved, and the conductivity is further improved; meanwhile, valence band change of the matrix is promoted, and the Seebeck coefficient is increased; in addition, due to the additional introduction of InBr3, the defects of the SnSe material are overcome, and the thermal conductivity in a full-temperature region is reduced; finally, collaborative optimization of high electrical transmission performance and low thermal transmission performance is achieved, and the problems that the electrical performance of N-type polycrystalline SnSe is low and it is difficult to synergistically improve the electrical transmission performance and the thermal transmission performance are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of thermoelectric materials, and in particular relates to a thermoelectric material based on N-type polycrystalline SnSe and a preparation method thereof. Background Art

[0002] Thermoelectric materials are a type of clean energy material that can be converted between thermal energy and electrical energy without the need for a fluid medium. They can achieve all-solid-state energy conversion and have the advantages of no noise, long service life, and good flexibility. At present, thermoelectric materials play an important role in power supply for deep space exploration and special military fields, cooling of 5G and even 6G communication chips, and cooling in the biomedical field (including medical thermostats, insulin coolers, and cold knives). Among them, SnSe-based thermoelectric materials have the characteristics of abundant reserves, environmental protection, low toxicity, low price, and low lattice thermal conductivity. They are considered to be a new type of medium-temperature thermoelectric material with great application potential.

[0003] Compared with P-type polycrystalline SnSe-based thermoelectric materials, the thermoelectric performance of N-type polycrystalline SnSe-based thermoelectric materials is relatively low, and there is still a lot of room for improvement, especially in terms of low electrical transmission performance. However, although the existing optimization methods for N-type polycrystalline SnSe-based thermoelectric materials can improve the electrical transmission performance of the material to a certain extent, the current electrical transmission performance is still at a relatively low level, and it is difficult to synergistically improve the electrical and thermal performance, resulting in its application is still limited. Therefore, it is necessary to develop new methods to optimize N-type polycrystalline SnSe thermoelectric materials to solve the problems of low electrical transmission performance of N-type polycrystalline SnSe and difficulty in synergistically improving electrical and thermal transmission performance. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings of the prior art, the present invention proposes a method for preparing a thermoelectric material based on N-type polycrystalline SnSe by using high-valent cation In 3+ and low-valent anions Br - The introduction of solves the problem of low electrical performance of N-type polycrystalline SnSe and difficulty in synergistically improving electrical and thermal transmission performance.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A first aspect of the present invention provides a thermoelectric material based on N-type polycrystalline SnSe, wherein the N-type polycrystalline SnSe thermoelectric material is an InBr3-doped SnSe material, and the molar ratio of Sn, Se, and InBr3 is (1-x):(0.93-3x):x, wherein 0<x≤0.0075.

[0007] Preferably, the molar ratio of Sn, Se and InBr3 is 0.995:0.915:0.005 or 0.9975:0.9225:0.0025 or 0.9925:0.9075:0.0075.

[0008] More preferably, the molar ratio of Sn, Se and InBr3 is 0.995:0.915:0.005.

[0009] This ratio can achieve the best synergistic optimization effect on the electrical and thermal transport performance of N-type polycrystalline SnSe thermoelectric materials, and its maximum power factor at 823K can reach 502μW m -1 ·K -2 , the thermoelectric figure of merit ZT reached 1.4.

[0010] The second aspect of the present invention provides a method for preparing the thermoelectric material based on N-type polycrystalline SnSe according to the first aspect, the preparation method comprising the following steps:

[0011] S1. Weigh Sn, Se, and InBr3 according to the composition ratio of the N-type polycrystalline SnSe thermoelectric material described in the first aspect;

[0012] S2. The symmetrical raw materials are melted to obtain N-type polycrystalline SnSe thermoelectric material.

[0013] The present invention uses high-valent cation In 3+ and low-valent anions Br - The introduction of InBr3 increases the carrier concentration and thus improves the electrical conductivity; at the same time, it also causes the matrix to achieve a valence band change and improves the Seebeck coefficient; in addition, the additional introduction of InBr3 increases the defects of the SnSe material, which reduces the thermal conductivity in the entire temperature range; ultimately achieving the coordinated optimization of high electrical transmission performance and low thermal transmission performance.

[0014] Preferably, Sn is ultrapure tin particles with a purity of ≥99.99%, Se is ultrapure selenium particles with a purity of ≥99.999%, and InBr3 is powder with a purity of ≥99.9%.

[0015] Raw materials (Sn, Se, InBr3) at this purity can reduce the introduction of impurities, thereby reducing the impact on thermoelectric performance.

[0016] Preferably, Sn, Se, and InBr3 are weighed in a glove box filled with 95% argon and 5% hydrogen, and the pressure value of the glove box is -4 to +4 Pa.

[0017] Operating in this atmosphere can prevent the raw materials from being oxidized, thereby preventing impurities from affecting performance.

[0018] Preferably, before the melting reaction, the raw materials are placed in a quartz tube in the order of Se, InBr3, and Sn; the inner diameter of the quartz tube is 15±0.2 mm, the wall thickness is 2±0.2 mm, and the inner wall of the quartz tube is evenly carbon-plated, and necking treatment is performed at a position about 100 to 130 mm from the bottom of the quartz tube.

[0019] Preferably, the quartz tube containing the raw materials is installed with a barrier valve in the glove box and then transferred to a tube sealing machine for vacuum treatment to a vacuum degree of less than 10 -4 Pa and then package; cut off the packaged quartz tube from the necking position to the tube mouth, then place it in a quartz tube with a diameter of 20±0.2mm and a wall thickness of 2±0.2mm that has been cleaned and dried with alcohol, and then evacuate and package it again.

[0020] Placing Se, InBr3, and Sn in the quartz tube in the order is conducive to the full reaction of the raw materials; using a quartz tube of this size can better protect the sample, and carbon plating the quartz tube can prevent the raw materials from reacting with the quartz tube, while further removing the inevitable residual oxygen during the melting reaction.

[0021] Preferably, during the melt reaction, the temperature is first raised to 950±50°C at a rate of 1.5-2°C / min, kept for 1440±60min for melt reaction, and then cooled to room temperature at a rate of 1.5-2°C / min; the obtained ingot is surface-polished using 1500-2500 mesh sandpaper and then hand-grinded using a mortar in a glove box for 30-50min.

[0022] The above-mentioned melt reaction process can ensure the acquisition of pure N-type polycrystalline SnSe, shorten the reaction time, increase efficiency, and allow the dopant to fully react with the matrix material. Grinding the ingot can effectively remove surface contaminants, and hand grinding in a mortar in a glove box can prevent the sample from being oxidized and mixed with water vapor.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention discloses an N-type polycrystalline SnSe thermoelectric material, namely, an InBr3-doped SnSe material, wherein the molar ratio of Sn, Se, and InBr3 is (1-x):(0.93-3x):x, wherein 0<x≤0.0075. 3+ and low-valent anions Br -The introduction of InBr3 increases the carrier concentration and thus improves the electrical conductivity; at the same time, it also causes the matrix to achieve a valence band change and improves the Seebeck coefficient; in addition, the additional introduction of InBr3 increases the defects of the SnSe material, which reduces the thermal conductivity in the entire temperature range; ultimately, the coordinated optimization of high electrical transmission performance and low thermal transmission performance is achieved, solving the problem of low electrical performance of N-type polycrystalline SnSe and difficulty in synergistically improving electrical and thermal transmission performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The test data spectrum of the conductivity of thermoelectric materials based on N-type polycrystalline SnSe varies with temperature;

[0026] Figure 2 This is a test data graph of Seebeck coefficient variation with temperature for thermoelectric materials based on N-type polycrystalline SnSe;

[0027] Figure 3 This is a test data graph of the power factor of thermoelectric materials based on N-type polycrystalline SnSe changing with temperature;

[0028] Figure 4 This is a test data graph of the thermal conductivity of thermoelectric materials based on N-type polycrystalline SnSe varying with temperature; Figure 5 This is a test data graph showing the change of thermoelectric figure of merit of thermoelectric materials based on N-type polycrystalline SnSe with temperature. DETAILED DESCRIPTION

[0029] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0030] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0031] Example 1: A thermoelectric material based on N-type polycrystalline SnSe and a preparation method thereof

[0032] (1) Three raw materials were weighed in a glove box filled with 95% argon and 5% hydrogen (pressure value was 1 Pa) according to the molar ratio of Sn:Se:InBr3=0.995:0.915:0.005, wherein Sn was ultrapure tin particles with a purity of ≥99.99%, Se was ultrapure selenium particles with a purity of ≥99.999%, and InBr3 was a powder with a purity of ≥99.9%.

[0033] (2) The raw materials are placed in a carbon-plated quartz tube in the order of Se, InBr3, and Sn. The quartz tube used has an inner diameter of 15±0.2 mm and a wall thickness of 2±0.2 mm, and is necked at a position of about 100 to 130 mm from the bottom of the quartz tube.

[0034] (3) Install a barrier valve on the quartz tube in the glove box, then transfer it to the tube sealing machine for vacuum treatment until the vacuum degree is less than 10 -4 Pa and then packaged.

[0035] (4) The packaged quartz tube is cut off from the necking position to the tube mouth, and then placed in a quartz tube with a diameter of 20±0.2mm and a wall thickness of 2±0.2mm (cleaned with alcohol and dried for 24 hours) for vacuumization and packaging again.

[0036] (5) The temperature was raised to 950±50°C at a rate of 1.5-2°C / min, and kept at that temperature for 1440±60min for melting reaction, and then cooled to room temperature at a rate of 1.5-2°C / min. After obtaining the ingot, the surface was polished with 2000-mesh sandpaper, and then hand-grinded with a mortar in a glove box for 40min.

[0037] (6) Pulse power-on pressure sintering is performed at a temperature of 500±50°C and a pressure of 50±5MPa for 10±3min to finally obtain an N-type polycrystalline SnSe thermoelectric material. The obtained N-type polycrystalline SnSe thermoelectric material is wire-cut and then polished into a suitable size for performance testing.

[0038] Embodiments 2-3: A thermoelectric material based on N-type polycrystalline SnSe and a preparation method thereof

[0039] The difference from Example 1 is that the molar ratios of Sn, Se and InBr3 in Examples 2 to 3 are different, wherein the molar ratio of Sn, Se and InBr3 in Example 2 is 0.9975:0.9225:0.0025; and the molar ratio of Sn, Se and InBr3 in Example 3 is 0.9925:0.9075:0.0075.

[0040] Comparative Example 1: A thermoelectric material based on N-type polycrystalline SnSe and a preparation method thereof

[0041] The difference from Example 1 is that in Comparative Example 1, InBr3 is replaced by InCl3, and the molar ratio of Sn, Se, and InCl3 is 0.995:0.915:0.005.

[0042] Experimental example: Performance test of thermoelectric materials based on N-type polycrystalline SnSe

[0043] Figure 1The test data of the conductivity variation with temperature of the thermoelectric materials based on N-type polycrystalline SnSe prepared in Examples 1 to 3 and Comparative Example 1 are reflected, and the conductivity is obtained by the conductivity Seebeck coefficient test system; Figure 2 The test data of Seebeck coefficient variation with temperature of the thermoelectric materials based on N-type polycrystalline SnSe prepared in Examples 1 to 3 and Comparative Example 1, wherein the Seebeck coefficient is obtained by a conductivity Seebeck coefficient test system; Figure 3 The test data of the power factor of the thermoelectric material based on N-type polycrystalline SnSe prepared in Examples 1 to 3 and Comparative Example 1 shows the change with temperature. The power factor (PF) is calculated by the conductivity (σ) and the Seebeck coefficient (S): PF = σ × S 2 ; Figure 4 The test data of the thermal conductivity of the thermoelectric materials based on N-type polycrystalline SnSe prepared in Examples 1 to 3 and Comparative Example 1 as a function of temperature are reflected. The thermal conductivity is calculated by combining the thermal diffusion coefficient (D) obtained by the laser thermal conductivity meter test, the density (ρ) obtained by the Archimedean drainage method test, and the Cp calculated by the Dulong-Petit law: κ = D × Cp × ρ; Figure 5 The test data of the thermoelectric figure of merit of the thermoelectric materials based on N-type polycrystalline SnSe prepared in Examples 1 to 3 and Comparative Example 1 show the change of the thermoelectric figure of merit with temperature. The thermoelectric figure of merit (ZT) is expressed by the power factor (S 2 It is calculated by multiplying the ratio of thermal conductivity (σ) to thermal conductivity (κ) by the absolute temperature (T).

[0044] Comprehensive analysis Figures 1 to 5 It can be seen that in the N-type InBr3-doped polycrystalline SnSe thermoelectric materials prepared in Examples 1 to 3, the high-valent cation In 3+ and low-valent anions Br - The introduction of In increases the carrier concentration and thus improves the conductivity. 3+ and Br - The introduction of also causes the matrix valence band to change and improves the Seebeck coefficient; in addition, the additional introduction of InBr3 increases the multi-scale defects in the SnSe material, which enhances phonon scattering and reduces the thermal conductivity over the entire temperature range. Among them, the solution of Example 1 is the best, but after InBr3 is replaced by InCl3 for the preparation of N-type polycrystalline SnSe thermoelectric material, the synergistic optimization effect of its electrical and thermal transport performance is significantly reduced. In addition, from Figure 1 It can be seen that the conductivity of the thermoelectric material of InCl3-doped N-type polycrystalline SnSe is much lower than that of Example 1, indicating that it is difficult for Cl ions to be doped into Se at the same ratio. 2- In the process, the power factor PF is not improved much, and the defects formed are relatively much lower, resulting in high thermal conductivity, which to a certain extent explains the irreplaceable nature of InBr3.

[0045] It can be seen that the method of the present invention can optimize the electrical and thermal transport properties of N-type polycrystalline SnSe thermoelectric materials at the same time. Moreover, it is precisely due to the coordinated optimization of electrical and thermal transport properties that the maximum power factor at 823K reaches 502μW m -1 ·K -2 , the thermoelectric figure of merit ZT reached 1.4.

[0046] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A thermoelectric material based on N-type polycrystalline SnSe, characterized in that: The N-type polycrystalline SnSe thermoelectric material is an InBr3-doped SnSe material, and the molar ratio of Sn, Se, and InBr3 is (1-x):(0.93-3x):x, wherein 0<x≤0.0075.

2. A thermoelectric material based on N-type polycrystalline SnSe according to claim 1, characterized in that: The molar ratio of Sn, Se and InBr3 is 0.995:0.915:0.005 or 0.9975:0.9225:0.0025 or 0.9925:0.9075:0.0075.

3. The method for preparing a thermoelectric material based on N-type polycrystalline SnSe according to claim 1 or 2, characterized in that: The following steps are involved: S1. Weigh Sn, Se and InBr3 according to the composition ratio of the N-type polycrystalline SnSe thermoelectric material according to claim 1 or 2; S2. The symmetrical raw materials are melted to obtain N-type polycrystalline SnSe thermoelectric material.

4. The method for preparing a thermoelectric material based on N-type polycrystalline SnSe according to claim 3, characterized in that: Sn is ultra-pure tin particles with a purity of ≥99.99%, Se is ultra-pure selenium particles with a purity of ≥99.999%, and InBr3 is powder with a purity of ≥99.9%.

5. The method for preparing a thermoelectric material based on N-type polycrystalline SnSe according to claim 3, characterized in that: Sn, Se, and InBr3 were weighed in a glove box filled with 95% argon and 5% hydrogen, and the pressure value of the glove box was -4 to +4 Pa.

6. The method for preparing a thermoelectric material based on N-type polycrystalline SnSe according to claim 3, characterized in that: Before the melting reaction, the raw materials are placed in a quartz tube in the order of Se, InBr3, and Sn; the inner diameter of the quartz tube is 15±0.2 mm, the wall thickness is 2±0.2 mm, the inner wall of the quartz tube is evenly carbon-plated, and a necking treatment is performed at a position about 100 to 130 mm from the bottom of the quartz tube.

7. The method for preparing a thermoelectric material based on N-type polycrystalline SnSe according to claim 3, characterized in that: The quartz tube with raw materials is placed in the glove box and then transferred to the tube sealing machine for vacuum treatment, so that the vacuum degree is less than 10 -4 Pa and then package; cut off the packaged quartz tube from the necking position to the tube mouth, then place it in a quartz tube with a diameter of 20±0.2mm and a wall thickness of 2±0.2mm that has been cleaned and dried with alcohol, and then evacuate and package it again.

8. The method for preparing a thermoelectric material based on N-type polycrystalline SnSe according to claim 3, characterized in that: During the melting reaction, the temperature is first raised to 950±50°C at a rate of 1.5-2°C / min, kept for 1440±60min for melting reaction, and then cooled to room temperature at a rate of 1.5-2°C / min; the obtained ingot is surface-polished with 1500-2500 mesh sandpaper and then hand-grinded with a mortar in a glove box for 30-50min.

Citation Information

Patent Citations

  • Polycrystalline SnSe2 low-cost thermoelectric material and preparation method thereof

    CN108396387A

  • N-type SnSe thermoelectric material and preparation method thereof

    CN108615806A

  • Preparation method of SnSe-based oriented polycrystalline thermoelectric material

    CN110098310A