Welded joint, welded member, method for producing same, and resistance spot welding method

By controlling the welding process in stages and adjusting the angle relationship, the problems of cracks and weld nugget diameter in resistance spot welding of galvanized steel plates were solved, achieving stable welding results under complex conditions, which is suitable for automotive parts.

CN119053402APending Publication Date: 2024-11-29JFE STEEL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380035310.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-03
Filing Date
2023-01-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During resistance spot welding of galvanized steel sheets, cracks are easily generated in the weld, especially shoulder cracks, and it is difficult to ensure the desired weld nugget diameter when the surface steel sheet thickness ratio and external interference are significant.

Method used

By adjusting the welding process, the welding process is divided into a first energizing step and a second energizing step. By controlling heat input and deformation, and by adopting specific angle and thickness relationships, combined with cooling and energizing modes, a weld nugget is formed and expanded in the intermediate stage, thus suppressing shoulder deformation and crack formation.

Benefits of technology

It effectively suppresses the formation of cracks in the weld, especially shoulder cracks, and stably ensures the desired weld nugget diameter, making it suitable for automotive parts, especially those exposed to rain.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053402A_ABST
    Figure CN119053402A_ABST
Patent Text Reader

Abstract

Provided is a welded joint in which at least one of the surface steel sheets of a sheet group is a zinc-plated steel sheet, cracks in a welded portion can be suppressed even when the thickness ratio of the surface steel sheets and the influence of external disturbance are large, and the welded joint has a nugget diameter of a desired size. The angle (a) of the shoulder in the first steel plate of the plate group and the angle (b) of the shoulder in the nth steel plate of the plate group satisfy at least one of formula (1) and formula (2).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a welding joint, a welding component and a manufacturing method thereof, and a resistance spot welding method. Background Art

[0002] In the assembly of automobiles, when overlapping steel plates are joined together, resistance spot welding, which is one of the overlapping resistance welding methods, is often used from the viewpoint of cost and manufacturing efficiency. Figure 1 As shown, a plate group 2 is formed by sandwiching steel plates 1-1 and 1-2 (hereinafter, the steel plate arranged at the upper side in the vertical direction is referred to as the upper electrode 3, and the electrode arranged at the lower side in the vertical direction is referred to as the lower electrode 4) and applying pressure from the upper and lower sides while passing welding current between the upper and lower electrodes to join the plates. In this welding method, a point-shaped weld is obtained by utilizing resistance heat generated by the flow of welding current. This point-shaped weld is referred to as a nugget 5. That is, the nugget 5 is a portion of the steel plate that melts and solidifies at the contact position of the steel plates when current flows through the overlapping steel plates. Using this nugget 5, the steel plates are joined to each other in a point shape.

[0003] In recent years, in the automotive field, the lightweighting of vehicle bodies has been developed to improve fuel consumption. As a result, the application of high-strength steel sheets in automotive parts is increasing. In addition, for parts of automotive parts that are suitable for parts exposed to rainwater, from the perspective of corrosion resistance, plated steel sheets (surface-treated steel sheets) with rust-proof properties such as zinc are used. Here, the plated steel sheet refers to a steel sheet with a metal coating on the surface of the parent material (base steel sheet). Examples of the metal coating include galvanized layers represented by electrogalvanizing and hot-dip galvanizing (including alloyed hot-dip galvanizing), zinc alloy coatings containing elements such as aluminum and magnesium other than zinc, and aluminum-zinc alloy coatings with aluminum and zinc as main components.

[0004] As a method suitable for resistance spot welding of a plate group formed by overlapping a plurality of steel plates including such a plated steel plate, for example, Patent Document 1 discloses the following method:

[0005] "A method for spot welding a high-strength plated steel sheet, characterized in that, in spot welding the high-strength plated steel sheet, the welding power-on time and the holding time after welding power-on are set in a manner that satisfies the following conditions (1) and (2), thereby spot welding is performed,

[0006] 0.25·(10·t+2) / 50≤WT≤0.50·(10·t+2) / 50··(1)

[0007] 300-500·t+250·t 2≤HT··(2)

[0008] Where, t: plate thickness (mm), WT: welding power-on time (ms), HT: holding time after welding power-on (ms)".

[0009] Patent Document 2 discloses the following method:

[0010] "A method for spot welding a high-tensile zinc-coated steel sheet, characterized in that when spot welding the high-tensile zinc-coated steel sheet using a multi-stage current supply of three or more stages, the welding conditions are adjusted so that the formed nugget has a desired nugget diameter d0 or more defined by the following formula (1) and a molten excess thickness of 0.05 mm or more,

[0011] d0=k√t………(1)

[0012] Here, d0: desired nugget diameter (mm)

[0013] k: coefficient; a coefficient between 3 and 6 that is selected to meet the construction conditions

[0014] t: Steel plate thickness (mm)".

[0015] Patent Document 3 discloses the following method:

[0016] "An electric welding method, characterized in that a plurality of overlapping steel plates are clamped and spot welded by opposed welding electrodes, wherein the plurality of overlapping steel plates include at least one steel plate coated with a coating at a welding position on at least one surface thereof,

[0017] Before spot welding, including the process of removing the coating,

[0018] In the above-mentioned process of removing the coating, the range of removing the coating is set at least within the circle of the outer edge of the welding heat-affected zone formed on the welding electrode side of the plurality of steel plates overlapping on the outer periphery.

[0019] Patent Document 4 discloses the following method:

[0020] "A spot welding method is a method of performing permanent welding of a welded part consisting of a plurality of steel plates overlapping at least the welding position by pressurizing and energizing the welding electrode, and further performing at least one of the energizing steps of front energization and rear energization, characterized in that:

[0021] For at least one of the plurality of steel plates, at least the overlapping surface of the welding position is coated with a zinc-based coating, and the total plate thickness t (mm) of the plurality of steel plates is 1.35 mm or more,

[0022] The welding electrodes are used to pressurize the parts to be welded from the start of the energization between the welding electrodes to the end of the energization between the welding electrodes at the end of welding.

[0023] When welding is completed, the post-energization holding time Ht (seconds) from the end of energization between the welding electrodes to the time when the welding electrodes and the welded member are out of contact is set within the range of the following formula (1):

[0024] 0.015t 2 +0.020≤Ht≤0.16t 2 -0.40t+0.70···(1)”.

[0025] Patent Document 5 discloses the following method:

[0026] "A resistance spot welding method is a method of joining a plurality of overlapping steel plates by clamping a pair of electrodes and applying pressure while passing electricity, wherein:

[0027] At least one of the plurality of overlapping steel plates is a surface-treated steel plate having a metal plating layer on the surface,

[0028] And, the following steps are included as the power-on process:

[0029] The main energizing process is to energize the nugget.

[0030] There is no energization process. After the main energization process, the energization is stopped for the energization stop time Tc (cycle).

[0031] The post-energization process is to conduct reheating without causing the nugget to grow after the non-energization process.

[0032] When the electrode travel angle (hitting angle) is set to A (degrees), the current value of the main energization process is set to Im (kA), the current value of the post-energization process is set to Ip (kA), 1+0.1·Tc is set to variable B, and 1+0.2·Tc is set to variable C, the above energization satisfies the relationship of the following formula (I),

[0033] Formula (I)

[0034] When 0<A<3, (22+A)·B / 100<Ip / Im<C

[0035] When 3≤A<7, (17+A)·B / 80<Ip / Im<C

[0036] When 7≤A<15, (11+A)·B / 60<Ip / Im<C”

[0037] Prior art literature

[0038] Patent Literature

[0039] Patent Document 1: Japanese Patent Application Publication No. 2003-103377

[0040] Patent Document 2: Japanese Patent Application Laid-Open No. 2003-236676

[0041] Patent Document 3: International Publication No. 2016 / 159169

[0042] Patent Document 4: Japanese Patent Application Publication No. 2017-47476

[0043] Patent Document 5: International Publication No. 2018 / 159764 Summary of the invention

[0044] However, in the resistance spot welding applied to a plate group formed by overlapping a plurality of steel plates including plated steel plates, particularly galvanized steel plates (hereinafter also referred to as resistance spot welding of galvanized steel plates), there is a problem that cracks are easily generated in the welded portion.

[0045] Generally speaking, the melting point of zinc coating and zinc alloy coating is lower than the melting point of the base material. Therefore, in the resistance spot welding of galvanized steel sheets, the low-melting-point metal coating on the surface of the steel sheet melts during the welding process. In addition, when the electrode pressure and the tensile stress caused by the thermal expansion and contraction of the steel sheet are applied to the weld, the molten low-melting-point metal invades the grain boundary of the base material of the galvanized steel sheet, thereby reducing the grain boundary strength and causing cracks. In other words, it can be considered that most of the cracks in the weld generated in the resistance spot welding of galvanized steel sheets are cracks caused by the so-called liquid metal embrittlement (hereinafter, also referred to as liquid metal embrittlement cracks).

[0046] Such liquid metal embrittlement cracks are likely to occur when a large deformation is applied to the weld. For example, when welding is performed under conditions that produce spatter, Figure 1 The surface of the plate group 1 connected to the welding electrodes 3 and 4 is prone to cracks. In particular, cracks generated at the outer peripheral portion of the contact area between the welding electrode and the plate group, that is, the shoulder portion of the plate group surface (hereinafter also referred to as shoulder cracks) are generated at a lower welding current value than cracks generated directly under the electrode.

[0047] On the other hand, from the viewpoint of ensuring the strength of the joint, it is important to ensure a nugget of a size greater than that specified. However, the greater the thickness ratio of the outermost steel plate (which contacts the electrode during welding) in the plate group (hereinafter also referred to as the surface steel plate), the more difficult it is to ensure a desired nugget diameter between the surface steel plate and the steel plate adjacent to the surface. Here, the thickness ratio of the surface steel plate refers to the value obtained by dividing the total thickness of the steel plates constituting the plate group by the thickness of the surface steel plate. In addition, during the construction during automobile assembly, when there is external interference during welding, for example, there is sometimes a gap between the fixed welding electrode and the plate group, and sometimes there is a gap between the steel plates of the plate group. In such a case, it is also difficult to ensure a desired nugget diameter.

[0048] In this regard, if the current value during welding is set to be large, the nugget diameter can be increased. However, if the current value during welding is set to be large, for example, a large deformation of the weld portion occurs due to the generation of spatter, and the risk of cracks in the weld portion, particularly liquid metal embrittlement cracks represented by shoulder cracks, increases.

[0049] In fact, in the techniques of Patent Documents 1, 2, 4 and 5, when the thickness ratio of the surface steel sheet and the influence of external disturbance are large, it is impossible to suppress the occurrence of cracks in the weld and stably ensure the desired size of the nugget diameter, and the current situation is that improvement in this regard is desired. It should be noted that improvement in this regard is also desired in resistance spot welding of galvanized steel sheets on steel sheets for other purposes, not only for automobile steel sheets.

[0050] In addition, in the technology of Patent Document 3, since a process of removing the plating layer on the surface of the steel plate in advance (hereinafter also referred to as a plating layer removal process) is required, the manufacturing cost is greatly increased. In addition, since the plating layer of the steel plate is removed, the corrosion resistance of the weld may also be reduced.

[0051] The present invention has been developed in view of the above-mentioned situation, and its purpose is to provide a welded joint, wherein at least one of the surface steel plates of the plate group is a galvanized steel plate, and even when the thickness ratio of the surface steel plate and the influence of external interference are large, cracks in the weld can be suppressed and the weld core diameter has a desired size.

[0052] In addition, the present invention aims to provide a resistance spot welding method for galvanized steel plates, which does not require a coating removal process and can simultaneously suppress the occurrence of cracks in the weld and stably ensure a desired nugget diameter even when the thickness ratio of the surface steel plate and the influence of external interference are large.

[0053] Furthermore, an object of the present invention is to provide a welded component having the above-mentioned welded joint and a method for manufacturing the same.

[0054] Therefore, the inventors have conducted intensive studies to achieve the above-mentioned object and have obtained the following findings.

[0055] Whether cracks in the weld, especially shoulder cracks, are generated during resistance spot welding of galvanized steel sheets has a great influence on the deformation of the shoulder of the plate group generated during welding, especially the shoulder angle. In addition, the shoulder angle is appropriately controlled based on the relationship between the tensile strength and thickness of the galvanized steel sheet configured as the surface steel sheet of the plate group (the steel sheet located on the outermost side of the plate group (in contact with the electrode during welding)), the total thickness of the steel sheets constituting the plate group, and the nugget diameter. Specifically, it is made to satisfy at least one of the equations (1) and (2) described later. In this way, the generation of cracks in the weld can be effectively suppressed.

[0056] Here, if Figure 2 As shown, the angle a of the shoulder in the first steel plate of the plate group (hereinafter, also referred to as the angle a of the shoulder) refers to the angle formed by the tangent of the shoulder of the first plate and the surface direction (the direction at right angles to the thickness direction, hereinafter also referred to as the surface direction) of the steel plates constituting the plate group on the cut surface in the thickness direction (hereinafter also referred to as the thickness direction) of the weld joint (plate group). Here, the tangent of the shoulder of the first plate refers to the tangent of the shoulder at the intersection point (hereinafter also referred to as the intersection point of the first plate) of the first straight line (hereinafter also referred to as the first straight line) parallel to the thickness direction passing through the end of the weld nugget and the shoulder surface of the first steel plate. In addition, as Figure 2 As shown in the figure, the angle b of the shoulder in the nth steel plate of the plate set (hereinafter also referred to as the angle b of the shoulder) refers to the angle between the tangent line of the nth shoulder and the surface direction on the cut surface in the thickness direction of the welded joint. Here, the tangent line of the nth shoulder refers to the tangent line of the shoulder at the intersection point of the first straight line and the shoulder surface of the nth steel plate (hereinafter also referred to as the intersection point of the nth sheet). Figure 2 In FIG. 1 , the angles a and b of the shoulder are shown by taking one end of the nugget (here, the end facing the right side of the paper) as a representative.

[0057] It should be noted that since the weld joint is basically axisymmetric at the center position of the nugget (the center position of the welding electrode during welding), the angles a and b of the shoulder can be measured at any cross section in the thickness direction of the weld joint passing through the center of the nugget (hereinafter also referred to as the cross section of the weld joint). However, when the angles a and b of the shoulder vary depending on the position (non-axisymmetric) such as when the welding electrode has a core shift or has a travel angle, the maximum values ​​thereof are set as the angles a and b of the shoulder, respectively.

[0058] In addition, due to deformation during welding, etc., when the surface direction is different depending on the steel plates constituting the plate group, the surface of the steel plate closest to the center position in the thickness direction of the plate group among the surfaces of the steel plates constituting the plate group is used as the reference surface, and the surface direction of the reference surface is used as the surface direction. In addition, due to deformation during welding, etc., when it is difficult to uniquely determine the surface direction of the steel plate, on the cut surface of the weld joint (when the angle of the shoulder is non-axisymmetric, the cut surface of the weld joint with the largest angle of the shoulder), the position 9 mm away from the center position of the weld nugget on the steel plate surface serving as the reference is used as the reference position. Then, the direction of the straight line connecting the reference positions can be set as the surface direction.

[0059] In addition, the nugget diameter W mentioned here refers to the long diameter (maximum diameter) of the nugget in the surface direction. That is, the nugget diameter W is measured, for example, on the cut surface of the weld joint as the distance between the ends of the nugget in the surface direction. Similarly, the diameter W0 of the intermediate stage nugget described later is the long diameter (maximum diameter) of the intermediate stage nugget in the surface direction. That is, the diameter W0 of the intermediate stage nugget is measured, for example, on the cut surface of the weld joint at the end of the first energization process, as the distance between the ends of the intermediate stage nugget in the surface direction.

[0060] In addition, spatter is one of the causes of deformation of the shoulder of the plate group generated during welding. Furthermore, cracks in the weld can be suppressed by suppressing the generation of spatter (the amount of molten metal that is scattered). Based on this, the inventors have conducted further repeated studies to obtain a resistance spot welding method that can suppress the generation of cracks in the weld and stably ensure a desired size of nugget diameter even when the thickness ratio of the surface steel plate and the influence of external disturbances are large.

[0061] As a result, the inventors have found that it is effective to satisfy the following (a) to (c) simultaneously.

[0062] (a) The current-carrying step during welding is divided into two steps: a first current-carrying step and a second current-carrying step.

[0063] (b) In the first energizing step, the energizing pattern is adjusted to control heat input, thereby forming an intermediate stage nugget (hereinafter also referred to as an intermediate stage nugget) while suppressing large deformation at the shoulder of the plate group as much as possible.

[0064] (c) In the second energizing step, by repeating the energizing and cooling pattern, the intermediate stage nugget is gradually enlarged while suppressing large deformation at the shoulder of the plate group as much as possible, thereby obtaining a nugget of a final size.

[0065] That is, in the first energizing step, it is necessary to finally form an intermediate stage nugget smaller than the target nugget in a manner that does not cause large deformation at the shoulder of the plate group in the second energizing step as a subsequent step. Therefore, it is important to adjust the energizing mode to control the heat input according to the thickness and tensile strength of the galvanized steel plate configured as the surface steel plate of the plate group and the total thickness of the steel plates constituting the plate group. It is particularly important to conduct energization under the condition that the diameter of the intermediate stage nugget formed in the first energizing step satisfies at least one of the equations (7) and (8) described later. Thus, it is possible to firmly form a crimping portion (plastic metal ring zone) around the intermediate stage nugget in the plate group as the object within the range required to ensure the final nugget diameter and suppress cracks in the weld. As a result, even when the thickness ratio of the surface steel plate and the influence of external interference are large, in the second energizing step, the intermediate stage nugget can be expanded while suppressing the amount of splashing. Thus, after the second energizing step is completed, a desired nugget diameter can be achieved while suppressing deformation of the shoulder portion of the plate assembly and even generation of cracks in the welded portion.

[0066] In addition, in the second energizing step, by energizing at a current value higher than the current value at the end of the energizing step in the first energizing step, the nugget can be enlarged in the intermediate stage. However, if the heat input is too large, a large deformation occurs at the shoulder of the plate group. Therefore, it is important to use an energizing pattern that repeats cooling and energizing for a fixed time or more. In this way, the nugget can be gradually enlarged while suppressing the large deformation at the shoulder of the plate group as much as possible.

[0067] The present invention has been completed through further studies based on the above findings.

[0068] That is, the main configuration of the present invention is as follows.

[0069] 1. A welded joint comprising a plate set consisting of n stacked steel plates and a nugget for joining the steel plates together,

[0070] n is an integer greater than or equal to 2,

[0071] In the plate set, at least one of the first steel plate and the nth steel plate from the top is a galvanized steel plate,

[0072] In the case of [Condition 1], the angle a of the shoulder portion in the first steel plate of the plate set satisfies the following formula (1):

[0073] In the case of [Condition 2], the angle b of the shoulder portion of the n-th steel plate of the plate set satisfies the following formula (2):

[0074] In the case of [Condition 3], the angles a and b of the shoulder satisfy the following equations (1) and (2), respectively:

[0075] In the above plate group, the diameter of the nugget x at the boundary level between the kth steel plate and the k+1th steel plate is k (mm) In the above, k is an integer from 1 to n-1, and t k is the thickness of the thinner steel plate between the kth steel plate and the k+1th steel plate (mm),

[0076] a≤{(980 / S U ) 0.3 ×(1 / T 0.3 )×(T / t U ) 0.2}×11×W 0.3 +15··· (1)

[0078] b≤{(980 / S L ) 0.3 ×(1 / T 0.3 )×(T / t L ) 0.2}×11×W 0.3 +15··· (2)

[0080] In the formula,

[0081] a: Angle of the shoulder of the first plate in the plate set (°),

[0082] b: Angle of the shoulder of the nth plate in the plate set (°),

[0083] T: Total thickness of n steel plates (mm),

[0084] t U : Thickness of the first steel plate (mm),

[0085] t L : The thickness of the nth steel plate (mm),

[0086] S U : Tensile strength of the first steel plate (MPa),

[0087] S L : tensile strength of the nth steel plate (MPa),

[0088] W: diameter of weld nugget (mm).

[0089] In addition, [Condition 1] to [Condition 3] are as follows.

[0090] [Condition 1]

[0091] Among the first steel plate and the nth steel plate of the plate set, only the first steel plate is a galvanized steel plate.

[0092] [Condition 2]

[0093] Among the first steel plate and the nth steel plate of the plate set, only the nth steel plate is a galvanized steel plate.

[0094] [Condition 3]

[0095] Of the first steel plate and the n-th steel plate in the plate set, both the first steel plate and the n-th steel plate are galvanized steel plates.

[0096] 2. The welded joint according to item 1 above, wherein:

[0097] In the case of the above [Condition 1], the angle a of the shoulder portion satisfies the following formula (3):

[0098] In the case of the above [Condition 2], the angle b of the shoulder portion satisfies the following formula (4),

[0099] In the case of the above-mentioned [Condition 3], the angles a and b of the above-mentioned shoulder portion satisfy the following equations (3) and (4), respectively.

[0100] a≤{(980 / S U ) 0.3 ×(1 / T 0.3 )×(T / t U ) 0.2}×6×W 0.3 +9··· (3)

[0102] b≤{(980 / S L ) 0.3 ×(1 / T 0.3 )×(T / t L ) 0.2}×6×W 0.3 +9··· (4)

[0104] 3. The weld joint according to item 1 or 2, wherein the total thickness T of the n steel plates and the thickness t of the first steel plate are U and the thickness t of the nth steel plate L At least one of the following equations (5) and (6) is satisfied.

[0105] T / t U >2···(5)

[0106] T / t L >2···(6)

[0107] 4. A welded component comprising the welded joint according to any one of 1 to 3 above.

[0108] 5. A resistance spot welding method, which is a method of joining a plate group consisting of n overlapping steel plates by clamping them with a pair of welding electrodes and applying pressure while passing electricity.

[0109] n is an integer greater than or equal to 2,

[0110] In the plate set, at least one of the first steel plate and the nth steel plate from the top is a galvanized steel plate,

[0111] In addition, the above resistance spot welding method has the following steps:

[0112] The first energizing step forms an intermediate nugget, and

[0113] The second power-on process expands the intermediate nugget.

[0114] In the first energizing step,

[0115] In the case of [Condition 1], power is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies the following formula (7):

[0116] In the case of [Condition 2], power is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies the following formula (8):

[0117] In the case of [Condition 3], power is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies both the following equations (7) and (8):

[0118] In the second energizing step, cooling in a non-energized state with a cooling time of 10 ms or more and less than 160 ms and energizing with a energizing time of 15 ms or more and less than 200 ms and a current value equal to or greater than the current value in the first energizing step are performed one or more times,

[0119] (T 0.3 / t U 0.2 )×(S U / 980) 0.1 ×2.0≤W0···(7)

[0120] (T 0.3 / t L 0.2 )×(S L / 980) 0.1 ×2.0≤W0···(8)

[0121] In the formula,

[0122] W0: diameter of the nugget in the middle stage (mm),

[0123] T: Total thickness of n steel plates (mm),

[0124] t U : Thickness of the first steel plate (mm),

[0125] t L : The thickness of the nth steel plate (mm),

[0126] S U : Tensile strength of the first steel plate (MPa),

[0127] S L : Tensile strength of the nth steel plate (MPa).

[0128] In addition, [Condition 1] to [Condition 3] are as follows.

[0129] [Condition 1]

[0130] Among the first steel plate and the nth steel plate of the plate set, only the first steel plate is a galvanized steel plate.

[0131] [Condition 2]

[0132] Among the first steel plate and the nth steel plate of the plate set, only the nth steel plate is a galvanized steel plate.

[0133] [Condition 3]

[0134] Of the first steel plate and the n-th steel plate in the plate set, both the first steel plate and the n-th steel plate are galvanized steel plates.

[0135] 6. The resistance spot welding method according to 5 above, wherein in the first energizing step,

[0136] In the case of the above [Condition 1], the current is applied under the condition that the diameter W0 of the nugget in the above intermediate stage satisfies the following formula (9):

[0137] In the case of the above [Condition 2], the current is applied under the condition that the diameter W0 of the nugget in the above intermediate stage satisfies the following formula (10):

[0138] In the case of the above-mentioned [Condition 3], the current is applied under the condition that the diameter W0 of the intermediate stage nugget satisfies both the following equations (9) and (10).

[0139] (T 0.45 / t U 0.3 )×(S U / 980) 0.15 ×2.0≤W0···(9)

[0140] (T 0.35 / t L0.3 )×(S L / 980) 0.15 ×2.0≤W0···(10)

[0141] 7. The resistance spot welding method according to 5 or 6 above, wherein in the first energizing step, energizing is performed under the condition of satisfying the following formula (11):

[0142] If>Is···(11)

[0143] In the formula,

[0144] Is: current value at the start of energization in the first energization step (kA),

[0145] If: Current value (kA) at the end of energization in the first energization step.

[0146] 8. The resistance spot welding method according to any one of 5 to 7 above, wherein the total thickness T of the n steel plates and the thickness t of the first steel plate are U and the thickness t of the nth steel plate L Satisfies at least one of the following (5) and (6).

[0147] T / t U >2···(5)

[0148] T / t L >2···(6)

[0149] 9. The resistance spot welding method according to any one of 5 to 8 above, wherein one or two or more of the following conditions (A) to (E) are satisfied.

[0150] (A) The welding electrode and plate assembly have a travel angle.

[0151] (B) A pair of welding electrodes produces core deviation.

[0152] (C) Before the plate pack is pressurized, there is a gap between the fixed welding electrode and the plate pack.

[0153] (D) Before the plate assembly is pressurized, a gap exists at at least one position between the steel plates of the plate assembly.

[0154] (E) On the surface of the plate assembly, the shortest distance from the center of the weld point to the end surface of the plate assembly is 10 mm or less.

[0155] 10. A welding method comprising the step of joining a plate set consisting of n stacked steel plates by the resistance spot welding method according to any one of 5 to 9 above, wherein n is an integer of 2 or more.

[0156] According to the present invention, a welded joint can be obtained, in which at least one of the surface steel plates of the plate group is a galvanized steel plate, and even when the thickness ratio of the surface steel plate and the influence of external interference are large, cracks in the weld can be suppressed and the weld core diameter has a desired size.

[0157] In addition, the welded part having the weld joint of the present invention is extremely suitable for automobile parts, especially automobile parts used in places exposed to rain, because the galvanized steel plate with high corrosion resistance is arranged on the outermost side. BRIEF DESCRIPTION OF THE DRAWINGS

[0158] Figure 1 It is a diagram schematically showing an example of the resistance spot welding method.

[0159] Figure 2 This is a diagram schematically showing an example of a cross section of a weld joint.

[0160] Figure 3 This is a diagram schematically showing an example of a plate group having plate gaps. DETAILED DESCRIPTION

[0161] The present invention will be described based on the following embodiments. First, a welded joint according to one embodiment of the present invention will be described.

[0162] [1] Welded joints

[0163] A welded joint according to one embodiment of the present invention comprises a plate set formed by stacking n steel plates and a nugget for joining the steel plates.

[0164] n is an integer greater than or equal to 2,

[0165] In the plate set, at least one of the first steel plate and the nth steel plate from the top is a galvanized steel plate,

[0166] In the case of [Condition 1], the angle a of the shoulder portion in the first steel plate of the plate set satisfies the following formula (1):

[0167] In the case of [Condition 2], the angle b of the shoulder portion of the n-th steel plate of the plate set satisfies the following formula (2):

[0168] In the case of [Condition 3], the angles a and b of the shoulder satisfy the following equations (1) and (2), respectively:

[0169] In the above plate group, the diameter of the nugget x at the boundary level between the kth steel plate and the k+1th steel plate is k (mm) In the above, k is an integer from 1 to n-1, and t kis the thickness of the thinner steel plate between the kth steel plate and the k+1th steel plate (mm),

[0170] a≤{(980 / S U ) 0.3 ×(1 / T 0.3 )×(T / t U ) 0.2}×11×W 0.3 +15··· (1)

[0172] b≤{(980 / S L ) 0.3 ×(1 / T 0.3 )×(T / t L ) 0.2}×11×W 0.3 +15··· (2)

[0174] In the formula,

[0175] a: Angle of the shoulder of the first plate in the plate set (°),

[0176] b: Angle of the shoulder of the nth plate in the plate set (°),

[0177] T: Total thickness of n steel plates (mm),

[0178] t U : Thickness of the first steel plate (mm),

[0179] t L : The thickness of the nth steel plate (mm),

[0180] S U : Tensile strength of the first steel plate (MPa),

[0181] S L : tensile strength of the nth steel plate (MPa),

[0182] W: diameter of weld nugget (mm).

[0183] In addition, [Condition 1] to [Condition 3] are as follows.

[0184] [Condition 1]

[0185] Among the first steel plate and the nth steel plate of the plate set, only the first steel plate is a galvanized steel plate.

[0186] [Condition 2]

[0187] Among the first steel plate and the nth steel plate of the plate set, only the nth steel plate is a galvanized steel plate.

[0188] [Condition 3]

[0189] Of the first steel plate and the n-th steel plate in the plate set, both the first steel plate and the n-th steel plate are galvanized steel plates.

[0190] Here, the plate group is formed by overlapping n steel plates, and at least one of the first steel plate and the nth steel plate counted from the top, that is, at least one of the surface steel plates of the plate group, is a galvanized steel plate. It should be noted that the order of counting from the top mentioned here can be, for example, the order of counting from the upper side in the vertical direction when the plate group is arranged in a manner that the surface of the plate group is parallel to the horizontal plane.

[0191] In addition, the galvanized steel sheet refers to a steel sheet having a zinc coating on one or both surfaces of a base steel sheet such as a hot-dip galvanized steel sheet or an alloyed hot-dip galvanized steel sheet. It should be noted that when a steel sheet having a zinc coating on one surface of a base steel sheet is used as the first steel sheet and the nth steel sheet, the zinc coating is preferably arranged in a manner that is located at the outermost side of the sheet group. Here, the zinc coating is a coating having a zinc content of 1% by mass or more, preferably a zinc content of 30% by mass or more. In the zinc coating, for example, in addition to the zinc coating such as a hot-dip galvanized layer, an alloyed hot-dip galvanized layer, and an electroplated galvanized layer, a zinc alloy coating containing alloy elements such as aluminum, magnesium, silicon, nickel, and iron in a total amount of less than 50% by mass is also included. In addition, as a zinc alloy coating (a steel sheet having a zinc alloy coating), for example, Galfan (Zn-5% by mass Al), Ecogal (registered trademark) (Zn-5% by mass Al-1% by mass or less of Mg and Ni) and the like can be cited. In addition, as the zinc alloy plating, there can also be cited an aluminum-zinc alloy plating containing a total of more than 67% by mass of aluminum and zinc and less than 33% by mass of alloying elements such as magnesium, silicon, nickel, and iron (for example, Galvalume (55% by mass Al-43.4% by mass Zn-1.6% by mass Si), etc.). In addition, the zinc-based plating preferably has a melting point lower than the melting point of the base steel sheet. In addition, the remaining components other than the above-mentioned zinc and alloying elements are unavoidable impurities. In addition, the base steel sheet is not particularly limited, and for example, steel sheets with various strengths ranging from mild steel with a tensile strength (hereinafter also referred to as TS): 270MPa grade to steel sheets with TS: 490 to 2500MPa grade can be applied.

[0192] In addition, the above-mentioned galvanized steel sheet can also be used for the steel sheets other than the first and n-th steel sheets in the steel sheet group. In addition, the uncoated steel sheet can also use steel sheets with various strengths, such as TS: 270MPa grade mild steel to TS: 490-2500MPa grade steel sheets. It should be noted that when the first steel sheet is a galvanized steel sheet, the n-th steel sheet can also use the above-mentioned galvanized steel sheet or the above-mentioned uncoated steel sheet. The same is true for the first steel sheet when the n-th steel sheet is a galvanized steel sheet.

[0193] The thickness of the steel plates constituting the plate set is not particularly limited, but is preferably 0.4 mm to 3.2 mm, for example. Steel plates having a thickness of 0.4 mm to 3.2 mm can be preferably used as automobile parts.

[0194] The number of stacked steel plates in the plate set, that is, n, may be an integer greater than or equal to 2. The upper limit of n is not particularly limited, and for example, n is preferably 7 or less.

[0195] Furthermore, in the welded joint of one embodiment of the present invention, as described above, it is important that the angle a of the shoulder in the first steel plate of the plate set and the angle b of the shoulder in the nth steel plate of the plate set satisfy at least one of the above equations (1) and (2) according to the above-mentioned [Condition 1] to [Condition 3]. It should be noted that the shoulder refers to Figure 2 The shoulder of the depression on the surface (front and back) of the plate group shown. In the figure, the symbols 1-1 to 1-3 are steel plates, 2 is a plate group, 5 is a nugget, and 6 is a shoulder. In addition, the depression on the surface (front and back) of the plate group mentioned here is a welding electrode mark caused by the pressure of the welding electrode during welding, and the nugget is located between the depressions.

[0196] Angles a and b of the shoulder portion: Based on the above-mentioned [Condition 1] to [Condition 3], at least one of the above-mentioned equations (1) and (2) is satisfied.

[0197] As described above, cracks in the weld generated during resistance spot welding of galvanized steel sheets, particularly cracks in the shoulder, are greatly affected by deformation of the shoulder of the plate assembly generated during welding, in other words, the angles a and b of the shoulder. Furthermore, by appropriately controlling the angles a and b of the shoulder based on the relationship between the tensile strength and thickness of the galvanized steel sheet arranged as the surface steel sheet of the plate assembly, the total thickness of the steel sheets constituting the plate assembly, and the nugget diameter W, cracks in the weld can be effectively suppressed.

[0198] Specifically,

[0199] Under the above-mentioned [Condition 1], the angle a of the shoulder satisfies the above formula (1),

[0200] In the case of [Condition 2] above, the angle b of the shoulder satisfies the above formula (2),

[0201] In the case of [Condition 3] above, the angles a and b of the shoulder satisfy the above equations (1) and (2), respectively.

[0202] This can effectively suppress the occurrence of cracks in the welded portion. It should be noted that the angles a and b of the shoulder portion and the method for measuring the nugget diameter W are as described above.

[0203] In addition, preferably,

[0204] Under the above-mentioned [Condition 1], the angle a of the shoulder satisfies the following formula (3):

[0205] In the case of the above-mentioned [Condition 2], the angle b of the shoulder satisfies the following formula (4),

[0206] In the case of the above-mentioned [Condition 3], the angles a and b of the shoulder satisfy the following equations (3) and (4), respectively. Thus, the generation of cracks in the weld can be more effectively suppressed, and in particular, the generation of tiny LME cracks with a shoulder length of less than 100 μm can be effectively suppressed.

[0207] a≤{(980 / S U ) 0.3 ×(1 / T 0.3 )×(T / t U ) 0.2}×6×W 0.3 +9··· (3)

[0209] b≤{(980 / S L ) 0.3 ×(1 / T 0.3 )×(T / t L ) 0.2}×6×W 0.3 +9··· (4)

[0211] In addition, the lower limits of the angles a and b of the shoulder portion are not particularly limited, and may be 0°. The angles a and b of the shoulder portion are preferably 1° or more, respectively.

[0212] In addition, it is preferable to satisfy at least one of the following formula (5) or formula (6). As described above, T / t U or T / t L In a large plate group, that is, a plate group in which the boundary between the steel plates constituting the plate group exists at a position away from the center position of the thickness of the entire plate group as the joined material (the position of 1 / 2 of the thickness of the plate group), it is sometimes difficult to ensure the size of the nugget. Therefore, when such a plate group is used, the effect of the present invention is more effectively exerted. Furthermore, it is preferable to suppress the occurrence of the crack in a plate group that satisfies at least one of the following formulas (12) or (13).

[0213] T / t U >2···(5)

[0214] T / t L >2···(6)

[0215] T / t U >3···(12)

[0216] T / t L >3···(13)

[0217] The diameter x of the nugget at the boundary level between the kth and k+1th steel plates k (mm): above

[0218] From the viewpoint of ensuring the joint strength, the nugget diameter x at the boundary level between the kth steel plate and the k+1th steel plate is set to k (mm) is set Above. Nugget diameter x k The upper limit of is not particularly limited, but from the viewpoint of suppressing the generation of spatter, the nugget diameter x k Preferably Here, k is an integer from 1 to n-1, t k is the thickness (mm) of the thinner steel plate among the k-th steel plate and the k+1-th steel plate. It should be noted that the nugget refers to a point-shaped welded portion where the steel plates of the plate set are joined together. In addition, the nugget is a portion formed by melting and solidifying the steel plates of the plate set.

[0219] [2] Welding parts

[0220] A welding component according to an embodiment of the present invention is a welding component having the above-mentioned welding joint. Since the welding component according to an embodiment of the present invention has a galvanized steel plate having high corrosion resistance arranged on the outermost side, it is suitable for automobile parts, especially automobile parts used in parts exposed to rainwater. It should be noted that in addition to the above-mentioned welding joint, the welding component according to an embodiment of the present invention may further have other welding joints (welding parts).

[0221] [3] Resistance spot welding method

[0222] A resistance spot welding method according to one embodiment of the present invention is a resistance spot welding method in which a plate group consisting of n stacked steel plates is sandwiched between a pair of welding electrodes and joined while applying pressure and electricity.

[0223] n is an integer greater than or equal to 2,

[0224] In the plate set, at least one of the first steel plate and the nth steel plate from the top is a galvanized steel plate,

[0225] In addition, the above resistance spot welding method has the following steps:

[0226] The first energizing step forms an intermediate nugget, and

[0227] The second power-on process expands the intermediate nugget.

[0228] In the first energizing step,

[0229] In the case of [Condition 1], power is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies the following formula (7):

[0230] In the case of [Condition 2], power is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies the following formula (8):

[0231] In the case of [Condition 3], power is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies both the following equations (7) and (8):

[0232] In the above-mentioned second energizing process, cooling in the non-energized state with a cooling time of more than 10 ms and less than 160 ms and energizing with a energizing time of more than 15 ms and less than 200 ms and a current value greater than the current value of the above-mentioned first energizing process are performed more than once.

[0233] (T 0.3 / t U 0.2 )×(S U / 980) 0.1 ×2.0≤W0···(7)

[0234] (T 0.3 / t L 0.2 )×(S L / 980) 0.1 ×2.0≤W0···(8)

[0235] In the formula,

[0236] W0: diameter of the nugget in the middle stage (mm),

[0237] T: Total thickness of n steel plates (mm),

[0238] t U : Thickness of the first steel plate (mm),

[0239] t L : The thickness of the nth steel plate (mm),

[0240] S U : Tensile strength of the first steel plate (MPa),

[0241] S L : Tensile strength of the nth steel plate (MPa).

[0242] In addition, [Condition 1] to [Condition 3] are as described above.

[0243] For example, Figure 1 As shown, a pair of welding electrodes 3 and 4 (upper electrode 3 and lower electrode 4) clamp the steel plates 1-1 and 1-2 (also called upper steel plate 1-1 and lower steel plate 1-2) to form a plate group 2, and pressurize them from the top and bottom while passing welding current between the upper electrode and the lower electrode to join. It should be noted that as a welding device that can be used in the resistance spot welding method of one embodiment of the present invention, as long as it has a pair of welding electrodes at the top and bottom, and can arbitrarily control the pressure and welding current during welding, the form (fixed setting, welding robot, etc.), electrode shape, etc. are not particularly limited. In addition, the structure for applying and controlling the pressure is not particularly limited, and previously known devices such as cylinders and servo motors can be used. Furthermore, the structure for supplying current and controlling the current value when energizing is not particularly limited, and previously known devices can be used. In addition, the current when energizing can also be any one of direct current and alternating current. It should be noted that in the case of alternating current, "current" refers to "effective current". The tip of the upper electrode 3 and the lower electrode 4 is not particularly limited, and examples thereof include DR type (dome spherical type), R type (spherical type), D type (dome type) and the like described in JIS C 9304: 1999. The tip diameter of the electrode is, for example, 4 mm to 16 mm.

[0244] In addition, in the resistance spot welding method of one embodiment of the present invention, as described above, the energizing process during welding is divided into two processes, namely, the first energizing process and the second energizing process. On this basis, in the first energizing process, the heat input is controlled by adjusting the energizing pattern, and the intermediate stage nugget is formed while suppressing the large deformation at the shoulder of the plate group as much as possible. In addition, in the second energizing process, the energizing pattern of energizing and cooling is repeated, and the intermediate stage nugget is gradually enlarged while suppressing the large deformation at the shoulder of the plate group as much as possible, and the nugget of the final size is obtained.

[0245] The first and second energizing steps are described below. It should be noted that the description of the plate set used in the resistance spot welding method according to one embodiment of the present invention is the same as the description of the plate set in the welded joint [1], and thus is omitted here.

[0246] ·The first power-on process

[0247] In the first energizing step, it is necessary to form a nugget in such a way that deformation does not occur at the shoulder of the plate group in the second energizing step as a subsequent step. Therefore, it is important to adjust the energizing mode to control the heat input according to the thickness and tensile strength of the galvanized steel sheet configured as the surface steel sheet of the plate group and the total thickness of the steel sheets constituting the plate group. It is particularly important to conduct energization under the condition that the diameter W0 of the intermediate stage nugget (the diameter of the nugget obtained at the end of the first energizing step) satisfies at least one of the above equations (7) and (8) according to the above [Conditions 1] to [Conditions 3].

[0248] Current supply conditions: According to [Condition 1] to [Condition 3], current is supplied when the diameter W0 of the intermediate stage nugget satisfies at least one of equation (7) and equation (8).

[0249] As described above, in the first energizing step, the energizing pattern is adjusted to control the heat input, and in particular, according to the above-mentioned [Condition 1] to [Condition 3], the energizing is performed when the diameter W0 of the intermediate stage nugget satisfies at least one of the above-mentioned formulas (7) and (8). As a result, it is possible to firmly form a crimping portion (plastic metal ring area) around the intermediate stage nugget within the range required to ensure the final nugget diameter and suppress cracks in the weld in the target plate group. As a result, even when the thickness ratio of the surface steel plate and the influence of external interference are large, in the second energizing step described later, the intermediate stage nugget can be expanded while suppressing the amount of splashing. As a result, after the second energizing is completed, the desired nugget diameter can be achieved on the basis of suppressing the deformation of the shoulder of the plate group and even the occurrence of cracks in the weld.

[0250] In addition, preferably,

[0251] In the case of the above-mentioned [Condition 1], power is supplied under the condition that the following formula (9) is satisfied,

[0252] In the case of the above-mentioned [Condition 2], power is supplied under the condition that the following formula (10) is satisfied,

[0253] In the case of [Condition 3] above, the current is applied under the conditions satisfying the following equations (9) and (10). This can more effectively suppress the occurrence of cracks in the welded portion. In particular, the occurrence of tiny LME cracks with a shoulder length of less than 100 μm can be effectively suppressed.

[0254] (T 0.45 / t U 0.3 )×(S U / 980) 0.15 ×2.0≤W0···(9)

[0255] (T0.35 / t L 0.3 )×(S L / 980) 0.15 ×2.0≤W0···(10)

[0256] In addition, the upper limit of the diameter W0 of the intermediate stage nugget is not particularly limited. If W0 becomes excessively large, the amount of spattering in the first energizing step may increase. Therefore, energizing is performed under the condition that the diameter W0 of the intermediate stage nugget is preferably W×0.9 mm or less, and more preferably W×0.8 mm or less. It should be noted that, as described above, W is the nugget diameter of the (finally obtained) weld joint (the diameter of the nugget at the end of the second energizing step).

[0257] If the power is applied under the condition that the diameter W0 of the molten metal in the intermediate stage satisfies the conditions in the above range (hereinafter also referred to as appropriate conditions), the other conditions are not particularly limited and can be applied according to conventional methods. It should be noted that the appropriate conditions vary depending on the plate group. In this regard, for example, a plate group identical to the plate group serving as the material to be joined is prepared, the current value of the first power-on process (hereinafter referred to as I1) is selected from the range of 2.0 to 15.0 kA, the power-on time is selected from the range of 15 to 2000 ms, and the applied pressure is selected from the range of 1.5 to 10.0 kN. Then, a pre-welding test is performed according to the various selected conditions. In this way, the appropriate conditions for each plate group can be obtained.

[0258] In addition, in the first energizing step, it is preferred to conduct energization in an uphill manner. For example, when the current value at the start of energization is set to Is (kA) and the current value at the end of energization is set to If (kA), it is preferred to satisfy the following formula (11). In this way, the effect of firmly joining the crimping portion (plastic metal ring area portion) around the nugget and the effect of forming a large intermediate stage nugget while suppressing deformation in the first energizing step can be more advantageously obtained.

[0259] If>Is···(11)

[0260] It should be noted that Is is preferably 2.0 to 14.0 kA, and If is preferably 3.0 to 15.0 kA.

[0261] When the current value changes during energization, the maximum current value in the first energization step (for example, the current value at the end of energization during the above-mentioned up-slope energization) is regarded as I1 (the current value in the first energization step).

[0262] · Second power-on process

[0263] In the second energizing step, the intermediate nugget formed in the first energizing step is gradually enlarged to obtain a nugget of a final size by repeating a energizing pattern of cooling and energizing while suppressing large deformation at the shoulder of the plate group as much as possible.

[0264] Cooling time: 10ms to 160ms in the non-powered state, and power-on time: 15ms to 200ms and current value: I1 or more: each performed at least once

[0265] As described above, in the second energizing process, it is necessary to gradually expand the intermediate stage nugget while suppressing the large deformation at the shoulder of the plate group as much as possible. Therefore, in the second energizing process, a energizing mode is set to repeatedly perform cooling and energizing. In particular, cooling in a non-energized state with a cooling time of more than 10 ms and less than 160 ms, and energizing with a energizing time of more than 15 ms and less than 200 ms and a current value of more than I1 are performed once or more. From the viewpoint of more advantageously obtaining the above-mentioned effects, the number of cooling and energizing is preferably more than 2 times, more preferably more than 3 times. It should be noted that if the number of cooling and energizing is greater than 10 times, the above-mentioned effect is saturated, and on the other hand, it sometimes leads to a decrease in construction efficiency. Therefore, the number of cooling and energizing is preferably less than 10 times, respectively.

[0266] In addition, in the above-mentioned cooling, if the cooling time each time is less than 10ms, sufficient cooling effect cannot be obtained. Therefore, large deformation is likely to occur at the shoulder of the plate group, and cracks are likely to occur in the weld. Therefore, the cooling time each time is set to be more than 10ms. In addition, from the viewpoint of gradually expanding the intermediate stage nugget while more advantageously suppressing large deformation at the shoulder of the plate group, the cooling time each time is preferably more than 15ms. On the other hand, if the cooling time each time is more than 160ms, the effect of expanding the intermediate stage nugget brought about by the power-on mode of repeatedly cooling and powering on may not be fully obtained. Therefore, the cooling time each time is set to be less than 160ms. The cooling time each time is preferably less than 120ms. It should be noted that cooling can be performed in a non-powered state, and the non-powered time is the cooling time.

[0267] Furthermore, in the above-mentioned energization, if the energization time of each time is less than 15ms, the intermediate stage nugget cannot be fully expanded in the second energization process due to insufficient heat input. Therefore, the energization time of each time is set to be more than 15ms. On the other hand, if the energization time of each time is more than 200ms, excessive heat input is applied by one energization, which is likely to cause large deformation of the weld part or even cracks. Therefore, the energization time of each time is set to be less than 200ms. The energization time of each time is preferably less than 160ms.

[0268] In addition, in the above-mentioned energization, in order to gradually expand the intermediate stage nugget, it is necessary to set the current value to be greater than I1, that is, to be greater than the current value of the first energization process. The current value in the above-mentioned energization is preferably greater than 1.1×I1. The upper limit of the current value in the above-mentioned energization is not particularly limited, but from the viewpoint of suppressing the generation of spatter, the current value in the above-mentioned energization is preferably less than 20kA.

[0269] It should be noted that the cooling time for each of the above cooling may be the same as or different from each other. In addition, the energization time and current value in the above energization are also the same.

[0270] There is no particular limitation on the conditions other than those mentioned above. Conventional methods can be used. For example, the pressure can be set to 1.5 to 10.0 kN. In addition, the pressure can be the same as that in the first power-on process, or it can be a different value. It should be noted that the current value during power-on can be fixed as long as it is above I1, or it can be appropriately changed during power-on, such as power-on in an uphill manner.

[0271] The conditions other than those mentioned above are not particularly limited and may be carried out according to conventional methods.

[0272] In addition, in the resistance spot welding method of one embodiment of the present invention, regardless of the influence of external disturbances and the plate group, the desired nugget diameter can be obtained while suppressing the occurrence of cracks in the weld. Therefore, the resistance spot welding method of one embodiment of the present invention is particularly suitable for strict welding conditions, such as when one or more of the following conditions (A) to (E) are satisfied.

[0273] (A) The welding electrode and plate assembly have a travel angle.

[0274] (B) A pair of welding electrodes produces core deviation.

[0275] (C) Before the plate group is pressurized, there is a gap between the fixed welding electrode and the plate group (hereinafter also referred to as the gap between the electrode and the plate group).

[0276] (D) Before the plate assembly is pressurized, a gap (hereinafter also referred to as a plate gap) exists at least at one position between the steel plates of the plate assembly.

[0277] (E) On the surface of the plate assembly, the shortest distance from the center of the weld point to the end surface of the plate assembly (hereinafter also referred to as the end surface shortest distance) is 10 mm or less.

[0278] Here, the "travel angle" of (A) refers to the angle of the axis of the welding electrode relative to the vertical direction of the surface of the plate group. In addition, "the state in which the welding electrode and the plate group have a travel angle" refers to the state in which the travel angle is not 0°, that is, the vertical direction of the surface of the plate group is not parallel to the axis of the welding electrode (at least one of the axis of the upper electrode and the axis of the lower electrode).

[0279] The "state in which a pair of welding electrodes is misaligned" in (B) refers to a state in which the axis of the upper electrode and the axis of the lower electrode of the welding electrode do not coincide with each other. The misalignment amount is the distance between the axis of the upper electrode and the axis of the lower electrode of the welding electrode.

[0280] The "before pressurization of the plate group" in (C) and (D) means after the plate group is set in a welding device having a fixed welding electrode (equivalent to the lower electrode in one example) and a driven welding electrode (equivalent to the upper electrode in one example) and before pressurization of the plate group is started by moving the driven welding electrode.

[0281] It should be noted that the resistance spot welding method according to one embodiment of the present invention is applicable not only to a plate set consisting of two stacked steel plates but also to a plate set consisting of three or more stacked steel plates.

[0282] [4] Method for manufacturing welded parts

[0283] A method for manufacturing a welded component according to an embodiment of the present invention is a method including the step of joining the plate set by the resistance spot welding method. Thus, it is possible to stably ensure a desired nugget diameter while suppressing deformation of the shoulder of the plate set and even generation of cracks in the welded portion. As a result, various welded components, particularly automobile components with a galvanized steel sheet having high corrosion resistance arranged on the outermost side, can be manufactured with high construction efficiency.

[0284] Example

[0285] For the plate groups shown in Table 1, resistance spot welding was performed under the conditions shown in Table 2 to produce welded joints. It should be noted that in each sample number, as shown in Table 1, external interference (welding conditions of (A) to (E) above) was simulated. In Table 1, "-" in the columns (A), (B), (C), and (E) means that the conditions are not satisfied. In addition, in the plate group simulating the plate gap of (D), such as in the group of three overlapping plates, Figure 3As shown, 30mm×100mm steel plates are overlapped, and 30mm×25mm gaskets 7 and 8 are sandwiched between the second and third steel plates to set a 2mm plate gap. It should be noted that "0mm" in the plate gap column of (D) means that there is no plate gap. In addition, in Table 1, for the samples marked "-" in the (E) column, the weld (nugget) is formed in a manner such that the center of the 30mm×100mm steel plate is the center of the weld point. In addition, in the first energization process, except for sample numbers 10, 21, and 22, energization is performed in an upslope manner. In sample numbers 10, 21, and 22, energization is performed at a fixed current value. The second energization process is performed in the order of cooling → energization, and each cooling and energization is performed under the same conditions.

[0286] In addition, the resistance spot welding was performed at room temperature and the welding electrode was always water-cooled. The upper electrode (driven welding electrode) and the lower electrode (fixed welding electrode) both used DR-type electrodes made of chromium copper with a front end diameter (front end diameter): 6 mm and a curvature radius: 40 mm. In addition, the pressure was controlled by driving the upper electrode with a servo motor, and a DC power supply was supplied when power was turned on. It should be noted that in all sample numbers, the plate group was configured in such a way that the first steel plate was in contact with the upper electrode (driven welding electrode).

[0287] For the welded joint thus obtained, the angles a and b of the shoulder of the plate set and the nugget diameter W were measured in the above-mentioned manner. Table 3 shows the results of these measurements.

[0288] In addition, for the obtained welded joint, the nugget diameter x1 at the boundary level between the first steel plate and the second steel plate was measured, and in the plate group of three steel plates, the nugget diameter x2 at the boundary level between the second steel plate and the third steel plate was further measured, and in the plate group of four steel plates, the nugget diameter x3 at the boundary level between the third steel plate and the fourth steel plate was further measured. These measurement results are shown in Table 3.

[0289] Furthermore, the surface and cross section of the nugget of the weld joint were observed to visually confirm the presence or absence of shoulder cracks. The results are also recorded in Table 3.

[0290] In addition, in Table 3, A, B and C in the column of shoulder crack have the following meanings.

[0291] A (Qualified, Excellent): No cracks

[0292] B (qualified): cracks are generated, but the length is less than 100 μm

[0293] C (failure): cracks with a length of 100 μm or more occur

[0294] In addition, in the judgment column in Table 3,

[0295] The shoulder crack is A, the core diameter is x k for The above situations are recorded as "qualified (excellent)".

[0296] The shoulder crack is B, the nugget diameter is x k for The above situation is recorded as "qualified (good)",

[0297] Cases other than the above, that is, cases where one of the target characteristics cannot be obtained, are recorded as "failed".

[0298] It should be noted that t1 is the thickness of the thinner steel plate of the first steel plate and the second steel plate. t2 is the thickness of the thinner steel plate of the second steel plate and the third steel plate. t3 is the thickness of the thinner steel plate of the third steel plate and the fourth steel plate. In addition, the nugget refers to a point-shaped welded portion where the steel plates of the plate set are joined to each other. In addition, the nugget is a portion formed by melting and solidifying the steel plates of the plate set.

[0299] Furthermore, another sample was prepared in which current was supplied to the first current supplying step under the same conditions as those of each sample number. Then, the diameter W0 of the intermediate nugget was measured in the above-mentioned manner in this sample. The measurement results are recorded in Table 2.

[0300]

[0301]

[0302]

[0303]

[0304]

[0305]

[0306] According to Table 3, in any of the inventive examples, it is possible to obtain a desired nugget diameter at each boundary level of the steel plate while suppressing the occurrence of cracks in the welded portion.

[0307] On the other hand, in Sample Nos. 17 and 25, since the second energizing step was not performed, that is, only one-stage energizing was performed, a desired nugget diameter could not be obtained depending on the boundary level of the steel plate.

[0308] In sample numbers 18 to 24, 33, 36, 37, 40, 43, 46 and 49, since power was applied when the diameter W0 of the weld nugget at the intermediate stage was not within the specified range in the first power-on process, cracks occurred in the weld, and the weld nugget diameter of the desired size could not be obtained depending on the boundary level of the steel plate.

[0309] In sample numbers 26 to 30, since the cooling time, current value, or energizing time in the second energizing step was outside the appropriate range, cracks occurred in the weld, or a desired nugget diameter could not be obtained depending on the boundary level of the steel plates.

[0310] Explanation of symbols

[0311] 1-1 Steel plate (upper steel plate)

[0312] 1-2 steel plate (lower steel plate)

[0313] 1-3 steel plate

[0314] 2-plate group

[0315] 3 welding electrode (upper electrode)

[0316] 4 welding electrode (lower electrode)

[0317] 5Nugget

[0318] 6Shoulders

[0319] 7. Gasket

[0320] 8. Gasket

Claims

1. A welded joint comprising a plate set consisting of n stacked steel plates and a nugget for joining the steel plates together, n is an integer greater than or equal to 2, In the plate set, at least one of the first steel plate and the nth steel plate from the top is a galvanized steel plate, In the case of condition 1, the angle a of the shoulder portion of the first steel plate of the plate set satisfies the following formula (1): In the case of condition 2, the angle b of the shoulder portion of the n-th steel plate of the plate set satisfies the following formula (2): In the case of condition 3, the angles a and b of the shoulder satisfy the following equations (1) and (2), respectively: In the plate group, the diameter x of the nugget at the boundary level between the kth steel plate and the k+1th steel plate is k =4.0√t k In the above, k is an integer from 1 to n-1, and t k is the thickness of the thinnest steel plate among the kth steel plate and the k+1th steel plate, x k and t k The unit is mm, a≤{(980 / S U ) 0.3 ×(1 / T 0.3 )×(T / t U ) 0.2 }×11×W 0.3 +15··· (1) b≤{(980 / S L ) 0.3 ×(1 / T 0.3 )×(T / t L ) 0.2 }×11×W 0.3 +15··· (2) In the formula, a: The angle of the shoulder in the first plate of the plate set, in degrees, b: The angle of the shoulder of the nth plate in the plate set, in degrees, T: Total thickness of n steel plates, in mm, t U : The thickness of the first steel plate, in mm, t L : The thickness of the nth steel plate, in mm, S U : The tensile strength of the first steel plate, in MPa, S L : The tensile strength of the nth steel plate, in MPa, W: diameter of weld nugget, in mm, In addition, conditions 1 to 3 are as follows. Condition 1 Of the first and nth steel plates in the plate set, only the first steel plate is a galvanized steel plate. Condition 2 Of the first and nth steel plates in the plate set, only the nth steel plate is a galvanized steel plate. Condition 3 Of the first steel plate and the n-th steel plate in the plate set, both the first steel plate and the n-th steel plate are galvanized steel plates.

2. The weld joint according to claim 1, wherein: In the case of condition 1, the angle a of the shoulder satisfies the following formula (3): In the case of condition 2, the angle b of the shoulder satisfies the following formula (4): In the case of condition 3, the angles a and b of the shoulder satisfy the following equations (3) and (4), respectively: a≤{(980 / S U ) 0.3 ×(1 / T 0.3 )×(T / t U ) 0.2 }×6×W 0.3 +9···(3) b≤{(980 / S L ) 0.3 ×(1 / T 0.3 )×(T / t L ) 0.2 }×6×W 0.3 +9···(4)。 3. The weld joint according to claim 1 or 2, wherein: The total thickness T of the n steel plates, the thickness t of the first steel plate U and the thickness t of the nth steel plate L Satisfies at least one of the following equations (5) and (6), T / t U >2···(5) T / t L >2···(6)。 4. A welded component comprising the welded joint according to claim 1 or 2.

5. A welded component comprising the welded joint according to claim 3.

6. A resistance spot welding method, which is a method of joining a plate group consisting of n overlapping steel plates by clamping them with a pair of welding electrodes and applying pressure while passing electricity. n is an integer greater than or equal to 2, In the plate set, at least one of the first steel plate and the nth steel plate from the top is a galvanized steel plate, In addition, the resistance spot welding method has the following steps: The first energizing step forms an intermediate nugget, and A second energizing step is performed to enlarge the intermediate stage nugget; In the first energizing step, In the case of condition 1, the current is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies the following formula (7): In the case of condition 2, the current is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies the following formula (8): In the case of condition 3, the current is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies both the following equations (7) and (8): In the second energizing step, cooling in a non-energized state with a cooling time of 10 ms or more and less than 160 ms and energizing with a energizing time of 15 ms or more and less than 200 ms and a current value greater than the current value of the first energizing step are performed at least once, (T 0.3 / t U 0.2 )×(S U / 980) 0.1 ×2.0≤W0···(7) (T 0.3 / t L 0.2 )×(S L / 980) 0.1 ×2.0≤W0···(8) In the formula, W0: The diameter of the molten core in the middle stage, in mm, T: Total thickness of n steel plates, in mm, t U : The thickness of the first steel plate, in mm, t L : The thickness of the nth steel plate, in mm, S U : The tensile strength of the first steel plate, in MPa, S L : The tensile strength of the nth steel plate, in MPa, In addition, conditions 1 to 3 are as follows. Condition 1 Of the first and nth steel plates in the plate set, only the first steel plate is a galvanized steel plate. Condition 2 Of the first and nth steel plates in the plate set, only the nth steel plate is a galvanized steel plate. Condition 3 Of the first steel plate and the n-th steel plate in the plate set, both the first steel plate and the n-th steel plate are galvanized steel plates.

7. The resistance spot welding method according to claim 6, wherein: In the first energizing step, In the case of the above condition 1, the current is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies the following formula (9): In the case of condition 2, power is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies the following formula (10): In the case of the condition 3, the current is applied under the condition that the diameter W0 of the nugget in the intermediate stage satisfies both the following equations (9) and (10): (T 0.45 / t U 0.3 )×(S U / 980) 0.15 ×2.0≤W0···(9) (T 0.35 / t L 0.3 )×(S L / 980) 0.15 ×2.0≤W0···(10)。 8. The resistance spot welding method according to claim 6, wherein: In the first energizing step, energizing is performed under the condition that the following formula (11) is satisfied: If>Is···(11) In the formula, Is: The current value at the beginning of the first energization process, in kA. If: Current value at the end of the first energization step, in kA.

9. The resistance spot welding method according to claim 7, wherein: In the first energizing step, energizing is performed under the condition of satisfying the following formula (11): If>Is···(11) In the formula, Is: The current value at the beginning of the first energization process, in kA. If: Current value at the end of the first energization step, in kA.

10. The resistance spot welding method according to claim 6, wherein: The total thickness T of the n steel plates, the thickness t of the first steel plate U and the thickness t of the nth steel plate L Satisfies at least one of the following (5) and (6), T / t U >2···(5) T / t L >2···(6)。 11. The resistance spot welding method according to claim 7, wherein: The total thickness T of the n steel plates, the thickness t of the first steel plate U and the thickness t of the nth steel plate L Satisfies at least one of the following (5) and (6), T / t U >2···(5) T / t L >2···(6)。 12. The resistance spot welding method according to claim 8, wherein: The total thickness T of the n steel plates, the thickness t of the first steel plate U and the thickness t of the nth steel plate L Satisfies at least one of the following (5) and (6), T / t U >2···(5) T / t L >2···(6)。 13. The resistance spot welding method according to claim 9, wherein: The total thickness T of the n steel plates, the thickness t of the first steel plate U and the thickness t of the nth steel plate L Satisfies at least one of the following (5) and (6), T / t U >2···(5) T / t L >2···(6)。 14. The resistance spot welding method according to any one of claims 6 to 13, wherein: Satisfies one or two or more of the following conditions (A) to (E), (A) The welding electrode and plate assembly have a travel angle, (B) A pair of welding electrodes produces core deviation, (C) Before the plate group is pressurized, there is a gap between the fixed welding electrode and the plate group. (D) Before the plate group is pressurized, there is a gap at least at one position between the steel plates of the plate group. (E) On the surface of the plate assembly, the shortest distance from the center of the weld point to the end surface of the plate assembly is 10 mm or less.

15. A method for manufacturing a welded component, comprising the step of joining a plate set consisting of n stacked steel plates by the resistance spot welding method according to any one of claims 6 to 13, wherein n is an integer of 2 or more. 16 . A method for manufacturing a welded component, comprising the step of joining a plate set consisting of n stacked steel plates by the resistance spot welding method according to claim 14 , wherein n is an integer greater than or equal to 2.

Citation Information

Patent Citations

  • Spot welding method for high strength plated steel plate

    JP2003103377A

  • Method for spot-welding high tensile strength galvanized base steel sheet

    JP2003236676A

  • Spot welding method

    JP2017047476A

  • Method for spot welding of plated steel sheet