Methods of configuring and manufacturing susceptors

By using easy-to-degradable receptors made by fusion of metal particles, the problems of slow drug activation and structural changes in the drug delivery route are solved, and safe aerosolization and environmentally friendly receptors of drugs are achieved at high temperatures, improving drug delivery efficiency and environmental safety sex.

CN119054414APending Publication Date: 2024-11-29CQENS TECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029901.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-04
Filing Date
2023-03-03
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing drug administration routes have many disadvantages, including slow activation of drugs in the digestive tract, potentially damaged, and causing side effects, aerosolization methods may change the molecular structure of the drug, and traditional receptor materials are not environmentally friendly and difficult to degrade.

Method used

Receptors made of metal particles fused, manufactured by sintering, direct metal laser sintering and other processes to form easily degradable receptors, and coat them on the surface of the receptor to increase environmental stability, ensuring that heating does not burn at high temperatures does not damage the drug. .

Benefits of technology

The aerosolization of drugs without burning at high temperatures has been achieved, which reduces changes in drug structure, improves the environmental protection and safety of receptors, and reduces the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119054414A_ABST
    Figure CN119054414A_ABST
Patent Text Reader

Abstract

A susceptor (106) for a heat-not-burn device (100) and a method of making the same, using metal pieces bonded together by various techniques such as compaction, heat and pressure, sintering, weaving, extrusion, etc. to form a single unitary piece, such that the susceptor is readily degraded after use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to methods for configuring and manufacturing susceptors, in particular devices for aerosolizing drugs via elevated temperatures. Background Art

[0002] When faced with a condition that causes physical discomfort (such as a disease state, illness, ailment, normal bodily disturbance, etc.), most people turn to medications, such as pharmaceuticals, supplements, herbs, etc., to immediately relieve the symptoms caused by the underlying condition. Certain legal and widely available over-the-counter (OTC) medications and supplements have beneficial effects when used for a variety of common conditions. Doctors also prescribe certain controlled narcotics and drugs for a variety of more serious conditions.

[0003] One of the most common routes of administration for these OTC and prescription drugs is oral administration. However, like any oral medication, it must pass through the digestive tract. There are many disadvantages to oral administration. For example, since the drug must pass through the digestive system, the activation of the drug begins slowly. In addition, in the digestive tract, the drug may be inactivated or destroyed and therefore lose its potency or efficacy. The drug itself may also cause digestive tract problems or side effects, such as loss of appetite, diarrhea, acidity, etc. In addition, patients may be unwilling or unable to swallow oral medications in pill form.

[0004] Certain drugs are intended to affect the brain or the actions or activities of the brain, but considering the accepted method of ingestion, i.e., gastrointestinal, intravenous, or intramuscular, these drugs may also produce various unpleasant side effects due to the nature of ingestion or injection. These include, but are not limited to, gastrointestinal complications, digestive disturbances, high blood pressure and / or headaches, as well as the user's reluctance to self-administer via injection.

[0005] There are other delivery routes, such as intradermal injection, patch application, inhalation, etc. Each of these has its own advantages and disadvantages. Therefore, there is still room for improvement in the route of drug administration.

[0006] For example, there are a variety of drugs that are safer, more potent, and more efficient in terms of safety and efficacy if their intake is via inhalation of an aerosol (e.g., gas, vapor, mist, and any other inhalant) containing the drug or its active ingredient rather than through gastrointestinal, intravenous, or intramuscular delivery.

[0007] Additionally, some methods of aerosolizing and delivering these drugs also have disadvantages, particularly those methods that aerosolize the drug itself, which alters the drug's molecular or chemical structure, or those methods that may perform aerosolization at elevated temperatures, which prolongs the duration of heating and increases the risk of altering the molecular or chemical structure of the active ingredient. Other disadvantages of current aerosolization technology include that some drugs are shipped, stored, and sold in cartridges that are prone to leakage, and in many cases, the design and construction materials of the cartridges are not environmentally friendly, containing plastics and other non-biodegradable materials.

[0008] To ensure intact drug delivery via a high temperature, non-combustion induction method, it is preferred that the aerosolization process does not change the chemical or basic molecular structure of the drug or other materials that make up the drug, or if such changes occur, they do not affect and / or improve the efficacy of the drug.

[0009] Therefore, there is still a need to improve the route of administration of medicine. In particular, there is still a need to improve the method for aerosolizing medicine so that it can be inhaled, which will also provide the additional benefit of metering, monitoring and measuring the precise dose of the inhaler without destroying the active ingredient or adding other chemicals to the aerosol due to low energy efficiency or extended heating time. There is also a need for consumable embodiments that are biodegradable and do not contain materials that do not meet environmentally friendly disposal.

[0010] In addition to drug delivery systems, heat-not-burn (HNB) devices are devices of the following type: generally used to heat tobacco at a temperature lower than that causing combustion to produce an aerosol containing nicotine and other tobacco components, which is then used by the user of the device. In some embodiments, a heated element or susceptor is placed inside a solid tobacco product, wherein a coil is wrapped around the tobacco product and the susceptor to heat the susceptor by an induction mechanism. Unlike traditional cigarettes, the goal is not to burn tobacco, but to fully heat tobacco to release nicotine and other components by producing an aerosol. Ignition and burning of cigarettes can produce undesirable toxins, which can be avoided by using HNB devices. However, it is difficult to balance between providing enough heat to effectively release tobacco components in the form of aerosol and not burning or igniting tobacco. HNB devices on the current market have not yet found this balance, either heating tobacco at a temperature that produces an inappropriate amount of aerosol, or overheating tobacco and producing an unpleasant or "burned" flavor distribution. In addition, current methods make the internal components of traditional HNB devices dirty by burning tobacco byproducts and byproducts of accidental combustion.

[0011] Furthermore, to ensure a rapid, energy-efficient change of state from a solid or liquid state to an aerosol state via high temperature, non-burning inductive heating, the formulation must be configured in a manner that eliminates air flow between the formulation and the inductive system susceptor. Thus, there is a need for a device, method, and formulation that provides the user thereof with the ability to control the power of the device, which will affect the temperature at which the tobacco is heated via an inductive method, thereby reducing the risk of combustion even at temperatures that would otherwise be sufficient to ignite, while increasing the efficiency and flavor profile of the generated aerosol.

[0012] These devices use an induction heating method where a susceptor embedded in an aerosol generating substrate is heated by a coil wrapped around the aerosol generating substrate and the susceptor. Current susceptors are typically made of a metal piece that may contain heavy metals such as lead, cadmium, etc. One problem with current susceptors is that, because they are flat pieces of metal, they may have very sharp edges and corners. Thus, if these devices or susceptors are not properly disposed of, they may become an environmental hazard similar to leaving razor blades scattered in the environment. Additionally, as solid metal pieces, current susceptors do not degrade quickly in the environment.

[0013] Therefore, there is a need for a susceptor and a method for manufacturing the same that is environmentally friendly and does not compromise the heat generation quality. Summary of the invention

[0014] The present invention relates to a method of configuring and manufacturing a susceptor that degrades in a relatively short period of time compared to standard susceptors made of metal alloys, particularly when the susceptor is exposed to a certain temperature. In particular, the susceptor may be composed of metal particles that are fused together so that the susceptor will decompose more easily when removed from a heat-not-burn device and exposed to the environment, thereby making the susceptor more environmentally friendly than other HNB susceptors that do not degrade and therefore become an environmental hazard.

[0015] In some embodiments, the metal particles can be fused together to form a metal sheet. The susceptor can be manufactured using a number of different fusion processes, such as using sintering, direct metal laser sintering, plasma spray powder, microwave assisted sintering, ultrasound assisted sintering, direct pressure, current assisted sintering, powder metallurgy, etc.

[0016] In some embodiments, the susceptor can be formed by weaving the "wire or wire" into a fabric-like sheet or strip, then cutting the sheet and using the sheet as a susceptor. This embodiment will also promote faster decomposition in the environment. These two embodiments feature a textured surface to create a larger surface area and optimize the adhesion of the substrate to the susceptor, simplify the consumable manufacturing process and ensure the tightest possible seal between the substrate and the susceptor, thereby achieving an induction heated high temperature non-burning consumable due to the lack of oxygen between the substrate and the susceptor.

[0017] In any embodiment, a protective coating on the susceptor may be used that burns off after the susceptor has been heated, making the susceptor more susceptible to rapid decomposition when removed from the heat-not-burn device and exposed to the environment. An example of a protective coating is a thin coating of PG sprayed with PGA to form a gel seal around the susceptor, thereby preventing the metal susceptor from oxidizing or decomposing until after it has been used. Any suitable coating may be used, but keep in mind that any aerosols generated by the heated coating may be inhaled by the user. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A side view showing the interior of an embodiment of the present invention assembled in an HNB device.

[0019] Figure 2A A perspective view of an embodiment of the present invention assembled into a consumable product containment package is shown.

[0020] Figure 2B Shows Figure 2A A perspective view of the embodiment shown with a portion of the consumable product containment package cut away and / or removed to expose the susceptor.

[0021] Figure 2C Shows Figure 2A The illustrated embodiment is a cross-sectional view taken along line 2C-2C.

[0022] Figure 2D Shows Figure 2A An exploded view of a consumable product containment package is shown.

[0023] Figure 2E A perspective view of another embodiment of a consumable product containing package having a susceptor is shown, with portions of the consumable product containing package cut away and / or removed to expose the susceptor.

[0024] Figure 3A A perspective view of another embodiment of a susceptor is shown.

[0025] Figure 3B Shows Figure 3A A side elevation view of a susceptor is shown.

[0026] Figure 3C Shows Figure 3A A top plan view of the susceptor is shown.

[0027] Figure 4A A perspective view of another embodiment of a susceptor is shown.

[0028] Figure 4B Shows Figure 4A A side elevation view of a susceptor is shown.

[0029] Figure 4C Shows Figure 4A A top plan view of the susceptor is shown.

[0030] Figure 5 Shows Figure 4A Close-up of the area marked 5 in FIG. DETAILED DESCRIPTION

[0031] The detailed description set forth below in conjunction with the accompanying drawings is intended as a description of an embodiment of the present invention and is not intended to represent that the present invention can be constructed or the only form of utilization. This description sets forth functions and step sequences for constructing and operating the present invention in conjunction with the embodiments shown. However, it should be understood that the same or equivalent functions and sequences can be realized by different embodiments, and these different embodiments are equally intended to be included in the spirit and scope of the present invention.

[0032] The invention of the present application is a susceptor 106 of a device for generating an aerosol from a consumable containing product for inhalation, which is generally referred to as a heat-not-burn (HNB) device 100, wherein the susceptor 106 becomes degradable after it has been used in the HNB device 100. The susceptor 106 is a component that is heated by an induction method and is used to heat the aerosol generating substrate 104 from the inside out. In this way, the susceptor 106 is made of a metal (such as a ferrous metal) that can be heated by an induction method. The HNB device 100 utilizes relatively high heat and minimizes the burning of the consumable containing product. The susceptor 106 of the present invention is configured to become degradable after being heated during the induction heating process when the HNB device 100 is used.

[0033] For the purposes of this application, the term "consumable" is broadly interpreted to cover any type of pharmaceutical agent, medicine, chemical compound, active agent, ingredient, any other drug, etc., regardless of whether the consumable is used to treat a condition or disease, for nutrition, is a tonic, or for recreation. By way of example only, consumables may include medicines, nutritional supplements, and over-the-counter drugs, such as, but not limited to, tobacco, tobacco raw materials, cigarettes, lavender, kava, coffee, caffeine, lobelia, cactus, melatonin, wolfberry, guarana, ginseng, etc.

[0034] Examples of HNB devices are Figures 1 to 2E The device 100 includes a consumable product containing package 102 and an aerosol generating device 200. The device 100 generates an aerosol by a heat-not-burn process, wherein the aerosol generating substrate 104 is exposed to an aerosolizing thermal state (such as a high aerosolizing temperature and the absence of oxygen) that does not burn the aerosol generating substrate 104 within the consumable product containing package 102, but does release the active ingredient from the aerosol generating substrate 104 in the form of an aerosol product that can be inhaled. Therefore, the aerosol generating substrate 104 is any product that contains an active ingredient that can be released in the form of an aerosol when heated to the appropriate temperature and conditions. Any description of the present invention to a specific application (such as tobacco products) is provided only as a specific example and is not intended to be limiting. Thus, the present invention is not limited to use with only tobacco products.

[0035] refer to Figure 1 The aerosol generating device 200 includes a receiving member 151 for receiving the consumable product containing package 102, an induction heating element 160 for heating the susceptor 106, a system controller for controlling the induction heating element 160, and a power supply 220 for powering the device 100. A user interface 230 may be provided for ease of operation. A trigger 232 may be provided to actuate the device 100.

[0036] The consumable product containing package 102 is a component that is heated to release the consumable product in the form of an aerosol. The consumable product containing package 102 includes an aerosol generating substrate 104 and a susceptor 106 surrounding the aerosol generating substrate 104 to heat the aerosol generating substrate 104 from the inside to the outside through an induction heating system. In some embodiments, the consumable product containing package 102 may have a shell 108 to contain the aerosol generating substrate 104 and the susceptor 106.

[0037] The shell 108 can be configured with holes 120 to allow aerosol to escape from the shell 108, or the shell can be a permeable membrane to allow aerosol to escape. The aerosol generating substrate 104 can be placed inside the housing 150 that can simulate a cigarette. In certain embodiments, the filter 140 can surround the shell 108. The housing 150 can be capped with an end cap 154 ​​at one end and capped with a suction nozzle 158 at the opposite end. The end cap 154 ​​can be made of a kind of filter material. The suction nozzle 158 allows the user to suck the heated consumable aerosol from the aerosol generating substrate 104 along the housing 150, toward the suction nozzle 158 into the user's mouth. Like this, the suction nozzle 158 can also include a kind of filter, similar to the end cap 154.

[0038] The invention of the present application is directed to a susceptor 106 that can be used in these and other HNB devices. Unlike prior art susceptors, which can be composed of a single solid piece of metal, the susceptors 106 of the present invention are configured to become degradable after they have been used in the HNB device 100. Thus, when prior art susceptors are discarded, they maintain their original form, which is often a flat rectangular piece of metal. Additionally, the edges of the flat rectangular piece of metal can be very sharp. Thus, if prior art susceptors are not properly disposed of, such as by wrapping in paper or tape or placing in a container for collecting sharp objects, sharp, razor-like susceptors can be introduced into the environment where they can cause harm to unsuspecting children, animals, and adults who may accidentally step on, pick up, or even ingest them.

[0039] However, the susceptor 106 of the present application is configured to be more environmentally safe than prior art susceptors. For example, the susceptor 106 can be made of a material that is a metal that is softer and more ductile than prior art susceptors and is therefore less likely to cause damage and / or have sharp edges. In some embodiments, the susceptor 106 can be made of a material that will degrade in a relatively short period of time (e.g., by oxidation). In some embodiments, the susceptor 106 can be configured to degrade or dissociate into smaller pieces when exposed to certain conditions, so that the susceptor is no longer a single integral piece, but a plurality of fragmented pieces. Therefore, the susceptor 106 may no longer be a single integral piece with hard or sharp features, but may become brittle in that the susceptor can be easily broken down into small pieces, crushed, or pulverized into a powder. In this way, when the degradable susceptor 106 is disposed of, it will be less harmful in the environment as it begins to degrade.

[0040] Examples of materials that can be used to make the susceptor 106 include, but are not limited to, any one or more of the following: iron or an iron-based alloy. Specifically, the susceptor can include about 50% to about 99.99% iron or an iron-based alloy. Preferably, the susceptor 106 can include about 98% or more iron or an iron-based alloy. In some embodiments, the susceptor 106 can include pure iron (100% iron).

[0041] Examples of conditions that may degrade the susceptor 106 include, but are not limited to, any one or more of the following: time, heat, pressure, sudden force, chemicals, water, etc. In a preferred embodiment, the susceptor 106 may become more fragile than current susceptors when exposed to the environment, even in the absence of heat. In this way, before its first use, the susceptor 106 may have structural integrity and rigidity, making it easy to handle during the manufacturing process of the HNB device 100, especially when the susceptor 106 is assembled with the aerosol-generating substrate 104. Once the susceptor 106 is incorporated into the aerosol-generating substrate 104 and inserted into the device 100, it is ready for use. During use, the susceptor 106 is heated to an aerosolization temperature, thereby releasing the active ingredient (drug) from the aerosol-generating substrate 104 in the form of an aerosol. The aerosolization temperature may be high enough to make the susceptor 106 brittle so that when the susceptor is removed from the heat-not-burn device and left in the environment, the susceptor may degrade. Since the aerosol-generating substrate 104 has already been used up in that area of ​​the susceptor 106, there is no impact on the user if the susceptor 106 becomes fragile in the used area.

[0042] In some embodiments, a coating may be applied to the susceptor 106 to protect the susceptor 106 from premature degradation until after the aerosol generating substrate has been used up. An example of this would be placing a coating of any one or more of propylene glycol (PG), vegetable glycerin (VG), polysorbate, paraffin, etc. on the metal susceptor 106, followed by adding a dusting material such as an alginate (e.g., propylene glycol alginate (PGA)) or any type of starch that can turn the coating (e.g., PG, VG, polysorbate, paraffin, etc.) into a gel to the susceptor 106. By way of example only, the ratio of coating to dusting material may be about 99:1 to convert the coating into a gel.

[0043] A variety of techniques can be used to create susceptors 106 that become brittle after use (or exposure to high aerosolization temperatures). Figures 3A to 5As shown, the degradable susceptor 106 may include a plurality of metal pieces 601 that are bonded together as a unitary piece. The susceptor 106 may be made of any metal material that generates heat when exposed to a changing magnetic field under induction heating. Ferromagnetic metals are preferred. In a preferred embodiment, when the temperature of the susceptor 106 of the present invention increases during use, the susceptor becomes more fragile and therefore more susceptible to degradation. Moreover, the protective coating on the susceptor will evaporate at the increased aerosolization temperature, thereby exposing the surface of the susceptor to more rapid degradation when exposed to the environment. By way of example only, the aerosolization temperature at which the susceptor 106 can be made fragile may be about 20 degrees Celsius to about 800 degrees Celsius. Preferably, the temperature at which the susceptor 106 can be made fragile may be about 40 degrees Celsius to about 600 degrees Celsius. More preferably, the temperature at which the susceptor 106 can be made fragile may be about 250 degrees Celsius to about 500 degrees Celsius. For example, the aerosolization temperature at which the susceptor 106 can be made fragile may be about 200 degrees Celsius to about 350 degrees Celsius. In some examples, the aerosolization temperature at which the susceptor 106 may be frangible may be about 40 degrees Celsius to about 150 degrees Celsius.

[0044] The shape of the susceptor 106 can be generally cylindrical, block-shaped, flat, etc., and can even be amorphous. Preferably, the unitary piece is a flat "sheet" comprising metal. In a preferred embodiment, the susceptor has a first end 600, a second end 602, and a surface 604 therebetween. Because the susceptor 106 includes a plurality of smaller pieces 601 (e.g., fragments, particles, metal shavings, metal powders, granules, fibers, strands, etc.), the surface 604 of the susceptor 106 may not be flat. Although the overall appearance of the surface 604 may appear to be flat or smooth, a closer inspection will reveal that the surface has a plurality of recesses and crevices, hills and depressions, and other undulations that create an uneven surface, such as Figure 5 As shown. The uneven surface also increases the total surface area compared to a smooth surface. Due to the unevenness, the surface 604 feels textured rather than smooth. The textured surface 604 increases the contact area with the aerosol generating substrate 104. In addition, the textured surface 604 can improve adhesion to the aerosol generating substrate 104. The uneven points on the surface 604 of the susceptor 106 can be embedded in the aerosol generating substrate 104. Embedding the uneven points in the aerosol generating substrate 104 increases the contact area between the susceptor 106 and the aerosol generating substrate 104. Allowing the aerosol generating substrate 104 to embed into the recesses and gaps of the surface 604 of the susceptor 106 eliminates oxygen between the susceptor 106 and the aerosol generating substrate 104.

[0045] The aerosol generating substrate 104 can be configured to minimize the amount of air to which the aerosol generating substrate 104 is exposed. This eliminates or reduces the risk of oxidation during storage or combustion during heating. Therefore, in certain settings, the aerosol generating substrate 104 can be heated to a temperature that will cause combustion when used with prior art devices that allow more air exposure. Thus, in some embodiments, the aerosol generating substrate 104 is made of a powdered form that is compressed into a hard compressed pellet or rod. The compression of the aerosol generating substrate 104 reduces the oxygen trapped in the aerosol generating substrate 104 and limits the migration and availability of oxygen in the aerosol generating substrate 104 during heating.

[0046] In some embodiments, the aerosol-generating substrate 104 and / or the susceptor 106 may be mixed with a substance that does not interfere with the function of the device 100 but displaces air in the interstitial space of the aerosol-generating substrate 104 and / or surrounds the aerosol-generating substrate 104 to isolate it from the air. For example, the substance may be an additive, such as a humectant, a flavoring agent, a filler for displacing oxygen, or a vapor-generating substance, etc. The additive may further aid in absorbing and transferring heat energy and eliminating oxygen from the aerosol-generating substrate 104. The additive may also serve as a corrosion inhibitor for the metal susceptor material.

[0047] In some embodiments, the susceptor 106 may be made of metal wool, such as Figure 2E For example, the susceptor 106 may be formed of metal wool filaments bundled together in a mat form. Thus, the metal wool mat includes a plurality of thin edges.

[0048] In some embodiments, the susceptor 106 may be impregnated, soaked or completely filled with additives, such as humectants, flavoring agents, vapor generating substances, substances that prevent oxidation of the susceptor 106, and / or fillers for eliminating air between the metal pieces 601, etc. There may be cutouts or gaps 112 along the susceptor 106 to divide the aerosol-generating substrate 104 into discrete segments for individually heated segments. Alternatively, individual susceptors 106 may be used that are separated by space and / or consumables so that each susceptor 106 can be individually heated during use.

[0049] In a preferred embodiment, the susceptor 106 may be made of a metal alloy such as mild steel. From an environmental standpoint, the advantages of mild steel include, but are not limited to, ease of disposal, as it begins to oxidize shortly after heating; thereby becoming brittle and easily degradable without dangerous sharp edges. Also, the metal, composed of iron and carbon, is relatively non-toxic.

[0050] However, alloyed metals may contain elements or chemicals that are considered hazardous (such as nickel, chromium, lead), and other metals that are undesirable if released into the environment or may be inhaled by a user. These elements may provide structural properties exhibited by alloys such as mild steel. However, since it is expected that the susceptor 106 will degrade after use, the susceptor 106 of the present application does not seek the kind of structural integrity used in prior art susceptors. Thus, in a preferred embodiment, the susceptor 106 has inferior structural properties (poor tensile, elastic, malleable and ductile properties) compared to prior art susceptors made of metal alloys. The susceptor 106 of the present invention can be made of a material that can quickly mechanically disintegrate (break apart) and chemically decompose (oxidize) if disposed of in the environment. A brittle susceptor 106 with lower structural integrity is desirable because, for example, it can reduce the risk of injury when accidentally ingested by or exposed to an animal or human.

[0051] In some embodiments, pure iron powder can be used as an excellent, low-cost, readily available ferromagnetic metal. When the particles are fused together, the iron alone has poor structural properties, but retains the excellent ferromagnetic properties required for induction heating. Without being bound by theory, it is believed that the metal pieces must be fused together at the boundaries of the particles to obtain the best possible susceptor performance. Thus, if FIG. 4A to FIG. 4C and Figure 5 As shown, the metal member 601 may be metal particles, metal shavings, metal powder, fibers, wire strands, etc., or any combination thereof that may be fused together.

[0052] In some embodiments, to fuse the metal pieces 601 together, a press may be used to compact the metal pieces 601. In some embodiments, the metal pieces 601 may be fused together by heat. In some embodiments, the metal pieces 601 may be fused together using heat and pressure (e.g., using a hot press). In some embodiments, the metal pieces 601 may be fused together using a binder (e.g., copper, paraffin, or other metallurgical binders). Preferably, a sintering process is used to fuse the metal pieces 601 together.

[0053] In some embodiments, direct metal laser sintering (DMLS) may be used. A smooth and flat "bed" of iron metal powder may be spread out on a flat surface. Using a laser, the shape of the desired susceptor may be drawn and filled in on the loose bed of metal powder. The laser cycles fuse the exposed particles together without completely liquefying all of the powder particles.

[0054] In a preferred embodiment, pure iron powder (i.e. 99.9% laboratory grade pure reduced iron) can be used. Other powdered metal types and alloys (mixtures) can also be used. For example only, in DLMS or other sintering processes, small iron pieces (such as iron powder or particles) can become small iron balls, which can enhance their induction heating design characteristics. Each of the iron balls can be fused together to form the shape of the susceptor 106. This shape can be designed by guiding the laser duration, power intensity, and the moving pattern of the laser beam. The roughness (i.e., surface texture) of the way in which the iron balls are fused together preferably provides an uneven and rough surface area for tobacco to adhere to the susceptor 106. Using powdered tobacco or other drugs compressed on the susceptor 106 with this rough surface area can provide better adhesion. After use (e.g., one-time heating), the susceptor 106 can be decomposed into small iron balls, which will degrade (rust) faster in the environment than traditional susceptors.

[0055] Laser speed, energy and frequency can all have different effects on surface finish, strength, thickness and speed of the sintering production cycle. Metal particle size (mesh) and shape can also affect the final surface finish and strength of the final susceptor product. Laser speed refers to the linear speed at which the beam moves across the surface of the powder bed. Laser energy refers to the optical power that the laser can deliver per unit time.

[0056] Metal particle sizes can range from 1 micron to about 2 mm in any given direction. An advantage of laser sintering metal powders is that by using different metal particle sizes, the porosity, density, and sensing characteristics of the fused susceptor can be controlled. Another advantage of sintered metal susceptors is that different particle sizes and shapes can be used, thereby allowing control of the rate at which the susceptor will degrade in the environment.

[0057] By way of example only, the power of the laser can be controlled to make the iron balls larger or smaller based on the intensity of the laser. The speed at which the laser travels on the surface of the small iron balls can be controlled to adjust the fusion strength of the bond between each of these balls. The movement of the laser can be controlled to adjust the shape (width, height, and length) of each susceptor 106, and the susceptors 106 can even be made in a specific pattern. For example, the susceptors 106 can be custom designed to form text or recognizable shapes, patterns, objects, animals, characters, etc. In addition, the shape of the susceptors 106 can be designed to improve the adhesion of the aerosol-generating substrate, such as forming a gap in the susceptor 106 so that the aerosol-generating substrate (e.g., powdered tobacco) can adhere to itself from both sides of the susceptor 106 through the gap.

[0058] The sintering process via laser is very fast, resulting in a susceptor 106 that is made cheaper than conventional susceptor manufacturing processes, while keeping the susceptor 106 pure, thereby avoiding the addition of any other harmful materials / alloys in the process. By optimizing the above factors, a susceptor 106 of ideal surface finish, strength and thickness can be produced. The finish of the susceptor 106 can be smooth to textured. Preferably, the surface is a textured finish to increase the contact surface area with the aerosol-generating substrate 104.

[0059] The thickness T of the susceptor 106 may range from about 1 micrometer to about 2 mm. Preferably, the thickness T of the susceptor 106 may range from 100 micrometers to 1.5 mm. More preferably, the thickness T of the susceptor may range from about 500 micrometers to 1 mm.

[0060] At the end of the laser sintering cycle, the fused susceptor 106 can be processed and removed from the surrounding loose unsintered powder bed, and the unsintered powder can be re-leveled for another sintering cycle. In some embodiments, an inert shielding gas (such as argon, nitrogen, carbon dioxide, or a mixture of gases) can be used to reduce oxidation during sintering. A wide variety of susceptor shapes and patterns can be designed and "drawn" on the powder bed by the engraving laser.

[0061] Infrared (IR) and ultraviolet (UV) wavelength lasers are capable of sintering metal particles. Lasers with other wavelengths of light can be used, as well as electron beam sintering.

[0062] In some embodiments, plasma spray powders can be used in the sintering process. Plasma spray powders are a process in which metal powders are superheated and sprayed through a plasma flame at high pressure toward a build surface, much like an inkjet printer sprays ink through an air gap onto the surface of a paper. The metal powder can be fed into the path of the plasma flame by a powder feeder. The plasma flame then heats the powder toward the build surface to create a susceptor.

[0063] Other sintering processes may be used, such as microwave sintering (in which a waveguide may be used to direct microwave energy into a chamber where metal particles rapidly fuse together), ultrasound-assisted sintering, direct pressure, current-assisted sintering, powder metallurgy (in which powders are pressed in the absence of heat to form a "green" state and then post-processed in a kiln or oven to fuse the particles together), etc.

[0064] In some embodiments, the susceptor 106 may be extruded by a machine. Once extruded, the aerosol-generating substrate 104 may be combined with the susceptor 106 by being compressed around the susceptor 106 along the length of the susceptor 106. Alternatively, the susceptor 106 may be stamped from flat metal stock or any other suitable manufacturing method before the aerosol-generating substrate 104 is assembled around the susceptor 106.

[0065] Preferably, the susceptor 106 is as thin as paper. Thus, the thickness T of the flattened susceptor 106 may be less than 0.1 inches (2.54 mm). Preferably, the thickness of the susceptor 106 may be less than 0.05 inches (1.27 mm). More preferably, the thickness of the susceptor 106 may be less than 0.025 inches (0.635 mm), or even less than 0.01 inches (0.254 mm). In some embodiments, the susceptor 106 may be as thin as 0.0039 inches (0.099 mm). The length of the susceptor 106 may range from about 0.5 inches (12.7 mm) to about 1.25 inches (31.75 mm). The length of the susceptor will vary based on the implementation of the device and its intended use in the heat-not-burn device. Thus, references in this application to smaller pieces 601 refer to fragments, particles, shavings, powders, granules, fibers, strands, etc., which individually have a total volume that is generally less than the total volume of the susceptor 106 being manufactured, so that the smaller pieces 601 are combined and fused to form the susceptor 106.

[0066] A variety of techniques may be used to obtain a thin, flattened susceptor 106, including sintering techniques. In some embodiments, the susceptor 106 may undergo a series of stretching and compression until the desired thickness T is reached. This may be achieved via rolling compression, followed by a stamping process to obtain the desired shape and texture, and other suitable methods. Once the desired thickness is reached, the susceptor 106 may be cut into the desired shape and size.

[0067] In certain embodiments, the use of steel wool for the susceptor and making the steel wool thin allows for easy and long-term cutting, as the blades used to cut the steel wool can last longer than conventional metal and thicker susceptors currently on the market. In addition, the use of steel wool is less expensive to manufacture and requires less energy to heat. In some embodiments, the energy required to bring other non-steel wool susceptors to the same temperature is reduced by about one-third. In some embodiments, the steel wool material used to make steel paper may require the addition of a lubricant when it is shaved into small wool materials. This may result in the addition of such lubricants to the finished steel wool material, resulting in reduced purity. In addition, steel wool made by shaving larger pieces of steel plates or steel rods may require the larger steel plates or steel rods to have a certain softness so that it can be shaved more easily. In order to make the steel softer, other alloys (such as lead) can be added to the steel plates or steel rods; however, the addition of other alloys reduces the purity of the steel. Such lubricants, alloys, or other materials used to produce such susceptors may be undesirable for heating and / or inhalation.

[0068] In some embodiments, the metal member 601 is an elongated metal fiber or strand. In this embodiment, the metal member 601 may be a low-grade carbon steel. FIG. 3A to FIG. 3C As shown, the metal fibers can be woven into a fabric-like sheet called steel fabric. The steel fabric has a textured surface 604 that increases the surface area, thereby optimizing heat transfer and adhesion to the aerosol-generating substrate 104 and eliminating oxygen between the susceptor 106 and the aerosol-generating substrate 104. The steel fabric can degrade over time, especially after it has been exposed to high aerosolization temperatures. Preferably, the steel fabric has sufficient ductility to bend and form into a fine screen. In order to make the fibers sufficiently ductile, alloys can be added to the steel; however, this reduces the purity of the susceptor 106.

[0069] Merely by way of example, a wire mesh weaving machine can be used to produce steel fabrics. In one example, the warp yarns (long threads extending along the length of the roll) are evenly spread and passed through two healds. Alternating threads pass through the front and rear healds. The weft threads extend over the width of the roll and pass through the warp threads when the loom is turned on. Each weft thread can be cut to the same length and wider than the desired width of the mesh roll being manufactured. The distance between the weft threads can be controlled by a reed mounted on a reciprocating beam, which pushes each weft thread into position. After positioning each weft thread, the front and rear heald threads travel to an upper position or a lower position depending on their previously positioned positions (upward or downward); the crossing of these warp threads captures the last weft thread in position.

[0070] This cycle is repeated until a length of woven mesh has been manufactured. After the weaving has taken place, the machine undergoes a calendering process. The calendering process passes the mesh through opposing rollers that are set to create the desired compression on the woven "material". Depending on the compression force applied, the strands of the mesh are crushed at the points where the warp and weft threads cross each other. These filaments then change from round filaments to a more oval cross-section. This changes the surface area of ​​the mesh, thereby reducing the space between the filaments without changing its mass. The calendering process also creates a more compact and robust "material".

[0071] After calendering, the web "material" is wound onto a rotating beam. The beam is then used to transport the "material" to the next process, slitting. The beam is placed in a slitter where the "material" is fed past several accurately positioned rotating blades that cut the wire mesh "material" into the exact width required. The slit material is wound onto a drum and then packaged.

[0072] A cleaning process as well as a drying and packaging process may be used to prevent any degradation / rusting of the material while shipping and storing (the rolls may also be wrapped in containers in an oxygen-free atmosphere).

[0073] The length of the aerosol-generating substrate (e.g., tobacco portion) minus the thickness of the aerosol-generating substrate can be specified at each end of the susceptor 106 to ensure that the complete encapsulation of the susceptor 106 will be produced. Before being fed into the aerosol-generating substrate manufacturing machine, the susceptor 106 material roll is inserted into the "susceptor preparation and testing machine", which unfolds and straightens the wire mesh "material", cleans it using several process cleanings, and finally cuts the material and crimps the material accurately to the specified width. Crimping prevents any strand from being lost. Cutting can be completed by rotating the cutter that is positioned to ensure cutting between the wefts to ensure that each final susceptor 106 has the same quality and electromagnetic characteristics. The final stage or preparation can involve electromagnetic inspection of each individual susceptor 106 by the machine to ensure that the features meet the specifications. The "good" susceptors 106 can be placed in a box, and the aerosol-generating substrate manufacturing machine will pick them up from the box.

[0074] The susceptor 106 preparation and testing machine may require an output speed of up to 20,000 pieces / minute, so there may be several rolls of susceptor material being unwound and processed in parallel. The first machine may have a lower output and may only need to process a single roll at a time, with a maximum of 5 rolls being processed in parallel. The most important function of the machine is to ensure the consistency and cleanliness of the susceptors 106.

[0075] Consistency can be achieved by providing material that meets physical and material specifications. Accurate cutting can be achieved by one of several methods, such as rotating self-sharpening knives and anvils or by rotating crimping. Delivery of only consistent susceptors 106 can be achieved by rotating electromagnetic coils and associated electronics to confirm the characteristics of the susceptor 106 entering the product.

[0076] The susceptor 106 may be delivered according to specifications including cleaning requirements and packaging specifications for the product of the roller. The susceptor 106 should be free of bacteria and organic material before being introduced into the aerosol generating substrate portion, and this may be achieved by a combination of: "washing" the unwinding roll, inductively heating the roll before it is unwound, and / or using known cleaning processes / techniques on the unwinding roll or elsewhere in the process.

[0077] The metals used in making the material can be different or the same, the wire diameter and shape can be different or the same. The product can be calendered to different degrees by varying the settings / pressure applied.

[0078] The disadvantages of the steel wool and steel fabric embodiments may be that they are too loose and the magnetic properties are not enough, making the heating process inefficient. To overcome these disadvantages, the steel wool or steel fabric susceptors can be fused together into a single, integrated fused metal sheet, for example, using a hot press to apply high temperature and high pressure. In some embodiments, the metal pieces 601 can be fused together without first weaving or interweaving (as in the case of steel fabric or steel wool) to form a so-called metal paper. The fused metal sheet has good magnetic properties and heats faster than when loosely interwoven or woven. However, in alternative embodiments, loose steel wool can be used for appropriate applications and induction power.

[0079] In any of the fused metal susceptor embodiments discussed herein, once the fused metal sheet is exposed to high temperatures, the fused metal sheet may lose its cohesion and become degradable (or demelt). Exposing the fused metal sheet to water after it has been heated may also corrode or degrade the metal sheet back to the metal piece 601 even faster. Additionally, the heated metal may oxidize more quickly after being heated, further accelerating degradation.

[0080] A surprising difference between using steel fabric and sintered susceptors is that steel susceptors 106 made via a sintering process tend to break down quickly and easily after heating. In one example, before use (i.e., heating), the susceptor 106 is a single, integral piece that can be held and compressed between ground tobacco under high pressure. However, after use (heating), the susceptor 106 breaks into small pieces of sandy, granular, or powdered material. Moreover, the iron particles can be rubbed between fingers and do not have any sharp edges.

[0081] In order to improve the uniformity, efficiency and consistency of the conduction of the susceptor 106, the manufacturing process should be able to repeatedly manufacture susceptors 106 with substantially the same characteristics (e.g., substantially the same density). For example, steel fabric has a consistent density due to the weave pattern. Steel wool material can achieve a consistent density through its compression and stretching stages. Loose metal pieces can be made into a consistent density using a magnetic drum. The magnetic drum can pick up the magnetic metal pieces 601 and discard the non-magnetic pieces. After collecting the magnetic metal pieces 601, they can be fed into a press to produce a uniform density. At the same time, the pressed metal pieces can be exposed to heat for a fusion process. In some embodiments, heat can be applied after being pressed.

[0082] When a susceptor 106 is formed, it may be exposed to a magnetic field and the electromagnetic induction characteristics of the susceptor 106 may be measured. Depending on the measured electromagnetic induction characteristics, a given susceptor 106 may be accepted or rejected when the susceptor 106 is produced. If a given susceptor 106 is rejected, the raw material may be adjusted during the manufacturing process (i.e., while the susceptor is being manufactured and produced) to produce a susceptor 106 whose magnetic characteristics meet the desired standards. In other words, the magnetic characteristics of the susceptor may be measured and adjusted simultaneously.

[0083] The electromagnetic induction properties of the susceptor 106 include, but are not limited to, the magnetic permeability and bulk resistance of its constituent materials. Without being bound by theory, it is believed that the susceptor 106 of the present application has improved electromagnetic induction properties over prior art susceptors because there are two mechanisms that contribute to induction heating: (1) hysteresis and (2) eddy current heating. Magnetic hysteresis requires the use of metals with high magnetic permeability, such as high purity iron. Eddy current heating relies on susceptor materials with high bulk resistance. By using a composition made of powdered, fragmented iron metal, the bulk resistance of the susceptor is greatly increased, thereby further increasing the heating effect from eddy currents. Some improvements of the susceptor 106 of the present application include, but are not limited to: using high purity iron with high magnetic permeability, constructing the susceptor from smaller pieces 601 (i.e., fragments, particles, powdered iron, etc.), and the fragmented surface structure of the susceptor further contributes to its bulk resistivity.

[0084] For the purpose of illustration and description, the above description of the preferred embodiments of the present invention has been presented. The above description is not intended to be exhaustive or to limit the present invention to the precise form disclosed. In view of the above teachings, many modifications and variations are possible. The scope of the present invention is not intended to be limited by this detailed description, but by the appended claims and their equivalents. Industrial Applicability

[0085] The present invention may be applied industrially to the development, manufacture and use of susceptors to improve the quality, manufacturing process and / or handling of susceptors that may be implemented in heat-not-burn devices (including other similar devices that use induction heating to aerosolize drugs for inhalation).

Claims

1. A susceptor comprising a plurality of metal parts joined together as an integral part, wherein: The monolithic piece is capable of degrading after use.

2. The susceptor according to claim 1, wherein: The metal member includes a carbon steel wire.

3. The susceptor according to claim 2, wherein: The unitary piece includes a weave pattern.

4. The susceptor according to claim 1, wherein: The metal part is a steel part.

5. The susceptor according to claim 4, wherein: The steel pieces are metal particles.

6. The susceptor according to claim 5, wherein: The steel pieces are fused together.

7. The susceptor according to claim 1, wherein: The metal member includes iron powder.

8. The susceptor according to claim 1, wherein: The monolith is configured to degrade upon being heated.

9. A method for manufacturing a susceptor, the method comprising: a) collecting multiple metal parts; b) combining the collected metal pieces into a unitary piece, thereby producing the susceptor, wherein the produced susceptor is configured to degrade when exposed to an aerosolization temperature.

10. The method of claim 9, further comprising flattening the unitary member into a flat sheet using a press.

11. The method of claim 9, wherein: The metal member is a carbon steel wire.

12. The method of claim 11, wherein: Combining the metal members into the unitary member includes braiding the carbon steel wires together.

13. The method of claim 12, wherein: Flattening the unitary piece further includes exposing the unitary piece to heat to fuse the metal pieces together to form the flattened sheet.

14. The method of claim 9, wherein: The metal pieces are collected by a magnetic drum.

15. The method of claim 14, wherein: Joining the metal pieces into a unitary flat sheet includes fusing the metal pieces together using pressure and heat.

16. The method of claim 15, wherein: After the susceptor is produced, the susceptor is exposed to a magnetic field to test the magnetic properties.

17. The method of claim 16, further comprising the steps of: The amount of the metal piece that is flattened in the press is adjusted based on the magnetic properties.

18. The method of claim 9, further comprising fusing the metal pieces together.

19. The method of claim 18, wherein: The metal parts are fused together by sintering.

20. The method of claim 19, wherein: The metal piece is sintered using a method selected from the group consisting of microwave sintering, ultrasound-assisted sintering, direct pressure sintering, current-assisted sintering, electron beam sintering, and powder metallurgy sintering.