Activating solution and activating method for SCR (Selective Catalytic Reduction) denitration catalytic module

By using activation solutions with components such as ammonium alumate, ammonium metatungstate and ammonium molybdate, combined with adsorbent solution of alcohol or carboxylic acid polymer compounds, the problem of reduced activity of SCR denitrification catalysts is solved, and efficient NOX conversion and catalytic effect are improved.

CN119056240AInactive Publication Date: 2024-12-03HEBEI QINGKAIQI ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411180798.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During use, the activity of existing SCR denitrification catalysts is reduced due to physical cleaning, excessive flue gas flow rate, alkali metal element reaction and heavy metal diffusion, and effective activation methods are needed to restore catalytic performance.

Method used

It adopts an activation liquid including a regeneration liquid and an adsorption liquid. The regeneration liquid consists of ammonium methyloltrium, ammonium metatungstate, ammonium molybdate and polyacrylamide. The adsorption liquid consists of alcohol or carboxylic acid polymer compounds. Coat evenly by spraying or soaking and calcining at 600-700°C to activate the catalyst.

Benefits of technology

It significantly improves NOX conversion rate and catalytic effect, ensuring the efficient operation of the SCR denitrification catalytic module.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to an activation solution and an activation method of an SCR (Selective Catalytic Reduction) denitration catalytic module. The activation solution comprises a regeneration solution and an adsorption solution, the regeneration liquid is prepared from 0.3 wt%-2 wt% of ammonium metavanadate, 0.9 wt%-6 wt% of ammonium metatungstate, 0.1 wt%-0.7 wt% of ammonium metamolybdate, 0.1 wt%-0.3 wt% of polyacrylamide and the balance water, and all the components of the regeneration liquid are distributed in a homogeneous phase mode in a solvent where the regeneration liquid is located; the adsorption liquid comprises polyvinyl alcohol or polyacrylic acid and the balance of water, the polyvinyl alcohol or polyacrylic acid is in homogeneous phase distribution in a solvent, and the SCR denitration catalytic module activated by the activation liquid of the SCR denitration catalytic module has the beneficial effects of high NOX conversion rate and good catalytic effect when being used for denitration of flue gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalyst activation, and in particular to an activation liquid and an activation method for an SCR denitration catalytic module. Background Art

[0002] Currently, the selective catalytic reduction of NH3 to remove NO x The method (SCR) has been widely used at home and abroad due to its high efficiency and mature technology. The catalyst used is mainly based on TiO2, with V2O5 as the main active ingredient, and WO3 or MoO3 as antioxidant and anti-poisoning auxiliary ingredients. The structure usually adopts honeycomb, plate and corrugated types.

[0003] During use, SCR denitration catalysts often fail due to the following reasons: 1. Multiple physical cleaning of the SCR denitration catalyst module causes the loss of the effective ingredient vanadium pentoxide. 2. The loss of the effective ingredient vanadium pentoxide due to excessive flue gas flow rate. 3. Alkali metal elements such as sodium and potassium directly react with the active area of ​​the catalyst. 4. Heavy metal elements, such as arsenic, diffuse into the catalyst and solidify in the active and inactive areas. 5. Alkaline earth metal elements, such as calcium, react with SO absorbed on the catalyst surface. X The reaction generates sulfate, which causes the catalyst surface to be covered. When the SCR denitration catalyst is poisoned, the catalytic activity will be greatly reduced, so it needs to be activated. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides an activated NO X Activation liquid and activation method for an SCR denitration catalytic module with high conversion rate and good catalytic effect.

[0005] The technical solution of the present invention is:

[0006] An activation liquid for an SCR denitration catalytic module comprises a regeneration liquid and an adsorption liquid; the regeneration liquid comprises 0.3-2wt% of ammonium metavanadate, 0.9-6wt% of ammonium metatungstate, 0.1-0.7wt% of ammonium metamolybdate, 0.1-0.3wt% of polyacrylamide, and the remainder is water, and the components of the regeneration liquid are uniformly distributed in the solvent; the adsorption liquid comprises polyvinyl alcohol or polyacrylic acid, and the remainder is water, and the polyvinyl alcohol or polyacrylic acid is uniformly distributed in the solvent.

[0007] Preferably, the solvent of the regeneration liquid is divided into two groups, A and B. The solvent of group A is used to dissolve polyacrylamide. The ammonium vanadate, ammonium metatungstate and ammonium metamolybdate are ground to at least 10,000 mesh and put into the solvent of group B to form a suspension. The suspension is evenly added to the solvent of group A for dissolving polyacrylamide, and stirring is continued until the ammonium vanadate, ammonium metatungstate and ammonium metamolybdate are dissolved.

[0008] In any of the above schemes, it is preferred that after the suspension is added, an alkaline pH regulator is introduced into the system until the pH value of the system is maintained at 11-12, and after the ammonium vanadate, ammonium metatungstate and ammonium metamolybdate are completely dissolved, an acidic pH regulator is added to the system until the pH value of the system is maintained at 7-8.

[0009] In any of the above schemes, preferably, the alkaline pH regulator is ammonia water, and the acidic pH regulator is an organic acid.

[0010] In any of the above schemes, preferably, the mass ratio of polyacrylamide to the solvent of group A is not greater than 0.5wt%;

[0011] In any of the above schemes, preferably, the regeneration liquid further includes 0.2-0.7 wt % of polyethylene glycol octyl ether and 1-1.2 wt % of cetylpyridinium bromide.

[0012] A method for activating an SCR denitration catalytic module, S1: mechanically cleaning the pores of a deactivated SCR denitration catalytic module;

[0013] S2: The adsorption liquid is evenly coated on the surface of the cleaned SCR denitration catalytic module pores by spraying or soaking;

[0014] S3: uniformly coating the regeneration liquid on the pore surface of the SCR denitration catalytic module treated in step S2 by spraying or soaking;

[0015] S4: calcining the SCR denitration catalytic module treated in step S3 at 600-700° C. for 1.5-2.5 hours.

[0016] Preferably, in step S2, the impregnated SCR denitration catalytic module is dried at 80-90° C. for 0.5-1 h.

[0017] In any of the above schemes, it is preferred that steps S2 to S4 are repeated according to the content of active components in the SCR denitration catalyst module.

[0018] Compared with the prior art, the activation liquid of the SCR denitration catalytic module of the present invention forms a relatively stable complex through the polyacrylamide in the regeneration liquid and the active ingredient precursors ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate; the alcohol polymer compound or carboxylic acid polymer compound in the adsorption liquid is stably combined with the TiO2 as the substrate at the pores of the SCR denitration catalytic module. During the activation process, the adsorption liquid is uniformly coated on the surface of the pores of the SCR denitration catalytic module in advance, and then the regeneration liquid is added. The polyacrylamide in the regeneration liquid and the active ingredients in the adsorption liquid are combined with each other through electrostatic interaction, hydrogen bonding, hydrophobic interaction and other mechanisms, so that the active ingredient precursors ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate are uniformly distributed on the surface of the pores of the SCR denitration catalytic module. The SCR denitration catalytic module is activated by calcining at 600-700°C. Therefore, the activated SCR denitration catalytic module has NO during denitration. X The beneficial effects are high conversion rate and good catalytic effect. DETAILED DESCRIPTION

[0019] The technical solution of the present invention will be described clearly and completely below in combination with the solution. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Embodiment 1:

[0021] In this embodiment, the solvent of the regeneration liquid is water. 5、 The ratio of WO3 and MoO3 is as follows: the concentration of ammonium metavanadate in the regeneration solution is 0.3-2wt%, the concentration of ammonium metatungstate is 0.9-6wt%, and the concentration of ammonium metamolybdate is 0.1-0.7wt%. Ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate are precursors of V2O5, WO3, and MoO3, respectively. The amide groups in polyacrylamide can form coordination with the empty orbits of the metal elements in ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate. The concentration of polyacrylamide is 0.1-0.3wt%, which ensures that the number of amide groups is sufficient and the effective dissolution of polyacrylamide is ensured. The regeneration liquid can be prepared by pre-dissolving polyacrylamide in a solvent, and after the polyacrylamide forms a homogeneous solution, adding ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate into the homogeneous solution of polyacrylamide according to the concentration of ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate, and continuously stirring. In order to increase the dissolution rate of polyacrylamide, a homogenizer can be used for stirring when dissolving the polyacrylamide. In order to increase the solubility of ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate, the system temperature can be increased to 50-70°C.

[0022] The adsorption liquid includes an alcohol polymer compound or a carboxylic acid polymer compound, and the solvent is water. The SCR denitration catalyst uses titanium dioxide as a substrate. It is understandable that titanium dioxide will interact with water molecules. The hydrogen atoms in the water molecules can form hydrogen bonds with the oxygen atoms on the surface of titanium dioxide, and then dissociate to produce hydroxyl groups on the surface. Secondly, the oxygen atoms on the surface of titanium dioxide have a certain reactivity and can easily capture hydroxide ions or hydrogen in water molecules from the environment to form hydroxyl groups. The crystal structure and surface defects of titanium dioxide will also affect the formation and distribution of hydroxyl groups. The unsaturated bonds and charge imbalance states at the surface defects will promote reactions with water molecules, etc., leading to the generation of hydroxyl groups.

[0023] The alcohol polymer compounds in the adsorption liquid can form a complex with titanium dioxide and adhere to the surface of the pores of the SCR denitration catalyst. The carboxylic acid polymer compounds in the adsorption liquid react with the hydroxyl groups on the surface of titanium dioxide through their carboxyl groups to achieve surface bonding with the pores of the SCR denitration catalyst.

[0024] In order to improve the solubility of the solute in the adsorption liquid and reduce the cost of manufacturing the adsorption liquid, the alcohol polymer compound is polyvinyl alcohol and the carboxylic acid polymer compound is polyacrylic acid.

[0025] When in use, the adsorption liquid is evenly coated on the pores of the SCR denitration catalyst module by spraying or infiltration in advance. Then the regeneration liquid is evenly coated on the pores of the SCR denitration catalyst module by spraying or infiltration. The alcohol polymer compound or carboxylic acid polymer compound adhering to the pores of the SCR denitration catalyst module combines with the polyacrylamide in the activation liquid through electrostatic interaction, hydrogen bonding, hydrophobic interaction and other mechanisms. As a result, the active ingredient precursor ammonium metavanadate and the antioxidant ingredient precursor ammonium metatungstate and ammonium metamolybdate are evenly and firmly distributed in the pores of the SCR denitration catalyst module. Finally, after high-temperature roasting at 600-700℃, the alcohol polymer compound or carboxylic acid polymer compound in the adsorption liquid and the polyacrylamide in the activation liquid are decomposed into water and carbon dioxide, and the ammonium metavanadate, ammonium metatungstate and ammonium metamolybdate in the activation liquid are converted into V2O5, WO3 and MoO3 respectively and evenly distributed in the pores of the SCR denitration catalyst module.

[0026] Compared with conventional activation solution, when the weight percentage of ammonium metavanadate, ammonium metatungstate and ammonium metamolybdate in the regeneration solution of the present invention is the same as that of conventional activation solution, the spraying amount or immersion time of the pores of the SCR denitration catalyst module is the same, and after being calcined at 600-700℃ for the same time, NO X The removal rate is shown in the following relationship:

[0027] Ammonium metavanadate: 0.3wt%, ammonium metatungstate: 0.9wt%, ammonium metamolybdate: 0.1wt%, polyacrylamide: 0.2wt%, NO X The removal rate is 90.77%.

[0028] Ammonium metavanadate: 0.3wt%, ammonium metatungstate: 0.9wt%, ammonium metamolybdate: 0.1wt%, oxalic acid: 5%, NO X The removal rate is 87.61%.

[0029] Ammonium metavanadate: 0.5wt%, ammonium metatungstate: 1.5wt%, ammonium metamolybdate: 0.16wt%, polyacrylamide: 0.2wt%, NO X The removal rate is 92.11%.

[0030] Ammonium metavanadate: 0.5wt%, ammonium metatungstate: 1.5wt%, ammonium metamolybdate: 0.16wt%, oxalic acid: 5%, NO X The removal rate is 90.36%.

[0031] Ammonium metavanadate: 0.7wt%, ammonium metatungstate: 2.1wt%, ammonium metamolybdate: 0.23wt%, polyacrylamide: 0.2wt%, NO X The removal rate is 94.06%.

[0032] Ammonium metavanadate: 0.7wt%, ammonium metatungstate: 2.1wt%, ammonium metamolybdate: 0.23wt%, oxalic acid: 5%, NO X The removal rate was 91.54%.

[0033] Ammonium metavanadate: 0.9wt%, ammonium metatungstate: 2.7wt%, ammonium metamolybdate: 0.3wt%, polyacrylamide: 0.2wt%, NO X The removal rate is 95.73%.

[0034] Ammonium metavanadate: 0.9wt%, ammonium metatungstate: 2.7wt%, ammonium metamolybdate: 0.3wt%, oxalic acid: 5%, NO X The removal rate is 92.24%.

[0035] Ammonium metavanadate: 1.1wt%, ammonium metatungstate: 3.3wt%, ammonium metamolybdate: 0.37wt%, polyacrylamide: 0.2wt%, NO X The removal rate is 94.89%.

[0036] Ammonium metavanadate: 1.1wt%, ammonium metatungstate: 3.3wt%, ammonium metamolybdate: 0.37wt%, oxalic acid: 5%, NO X The removal rate is 92.94%.

[0037] Ammonium metavanadate: 1.3wt%, ammonium metatungstate: 4.5wt%, ammonium metamolybdate: 0.5wt%, polyacrylamide: 0.2wt%, NO X The removal rate was 95.46%.

[0038] Ammonium metavanadate: 1.3wt%, ammonium metatungstate: 4.5wt%, ammonium metamolybdate: 0.5wt%, oxalic acid: 5%, NO X The removal rate is 93.25%.

[0039] Ammonium metavanadate: 2wt%, ammonium metatungstate: 6wt%, ammonium metamolybdate: 0.7wt%, polyacrylamide: 0.2wt%, NO X The removal rate is 95.53%.

[0040] Ammonium metavanadate: 2wt%, ammonium metatungstate: 6wt%, ammonium metamolybdate: 0.7wt%, oxalic acid: 5%, NO X The removal rate was 94.59%.

[0041] Among them, NO X The calculation formula of the removal rate R is:

[0042]

[0043] In the formula, NO Xin is the NO at the inlet of the SCR denitration catalyst during actual testing X Concentration, NO Xout is the NO at the outlet of the SCR denitration catalyst during actual testing X concentration.

[0044] Embodiment 2:

[0045] On the basis of Example 1, in order to improve the dissolution rate of ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate in the regeneration liquid, and the uniformity in the system after dissolution. In this embodiment, the solvent of the regeneration liquid is divided into two groups, A and B, and polyacrylamide is dissolved in the solvent of group A. Grind ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate to at least 10,000 mesh to increase the specific surface area of ​​each substance, and then put the three ground substances into the solvent of group B to form a suspension, and evenly add the suspension to the solvent of group A in which polyacrylamide is dissolved, and continue stirring until the ammonium metavanadate, ammonium metatungstate, and ammonium metamolybdate are dissolved. Among them, in order to effectively dissolve polyacrylamide, the mass ratio of polyacrylamide to the solvent of group A is not more than 0.5wt%;

[0046] In this embodiment, after the suspension is added, an alkaline pH regulator is introduced into the system until the pH value of the system is maintained at 11-12. In an alkaline environment, the concentration of hydroxide ions is relatively high. These hydroxide ions can interact with tungstate ions, vanadate ions, and molybdate ions in the system, changing their ion form and charge distribution, thereby making them more soluble.

[0047] After the ammonium metavanadate and ammonium metatungstate are completely dissolved, an acidic pH regulator is added to the system to maintain the pH value of the system at 7-8 to ensure that when the SCR denitration catalyst is regenerated, the polyacrylamide in the regeneration liquid can better react with the alcohol polymer compound or carboxylic acid polymer compound in the adsorption liquid.

[0048] When adjusting the pH value of the system, in order to prevent the introduction of metal ions and inorganic acid radicals from affecting the performance of the SCR denitration catalyst, the alkaline pH regulator can be ammonia water, and the acidic pH regulator can be an organic acid, so as to ensure that the alkaline pH regulator and the acidic pH regulator introduced can be removed during the calcination stage at 600-700°C when the SCR denitration catalyst is activated.

[0049] Embodiment 3:

[0050] On the basis of Example 1 or 2, in order to prevent the agglomeration of ammonium metavanadate, ammonium metatungstate and ammonium metamolybdate in the regeneration liquid in the system, so as to make the distribution of ammonium metavanadate, ammonium metatungstate and ammonium metamolybdate in the system more uniform, a dispersant is further added to the regeneration liquid, and the dispersant includes 0.2-0.7wt% of polyethylene glycol octyl ether and 1-1.2wt% of cetylpyridinium bromide.

[0051] Embodiment 4:

[0052] Based on any one of Examples 1-3, this embodiment provides a method for activating an SCR denitration catalytic module, the method comprising the following steps:

[0053] S1: Mechanically clean the pores of the deactivated SCR denitration catalytic module;

[0054] S2: The adsorption liquid is evenly coated on the surface of the cleaned SCR denitration catalytic module pores by spraying or soaking;

[0055] S3: uniformly coating the regeneration liquid on the pore surface of the SCR denitration catalytic module treated in step S2 by spraying or soaking;

[0056] S4: calcining the SCR denitration catalytic module treated in step S3 at 600-700° C. for 1.5-2.5 hours.

[0057] The mechanical cleaning in step S1 includes at least one of acid cleaning, alkaline cleaning, ultrasonic cleaning and water cleaning.

[0058] Embodiment 5:

[0059] On the basis of Example 4, in order to enhance the bonding strength between polyacrylamide in the regeneration liquid and alcohol polymer compounds or carboxylic acid polymer compounds in the adsorption liquid, in step S2, the SCR denitration catalytic module with the adsorption liquid uniformly coated on the pore surface is dried at 80-90°C for 0.5-1h to partially remove the moisture in the adsorption liquid coated on the surface of the SCR denitration catalytic module.

[0060] Embodiment 6:

[0061] Based on Example 4 or 5, the SCR denitration catalytic module is used to denitrate NO X The experimental data of the removal rate is fed back, or the results of the quantitative detection of the contents of vanadium, titanium, tungsten and molybdenum on the surface of the pores of the SCR denitration catalytic module are repeated, and steps S2-S4 are repeated.

[0062] The embodiments described above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An activation solution for an SCR denitration catalytic module, characterized in that: Including regeneration liquid and adsorption liquid; The regeneration liquid comprises 0.3-2wt% of ammonium metavanadate, 0.9-6wt% of ammonium metatungstate, 0.1-0.7wt% of ammonium metamolybdate, 0.1-0.3wt% of polyacrylamide, and the rest is water, and the components of the regeneration liquid are uniformly distributed in the solvent; The adsorption liquid includes polyvinyl alcohol or polyacrylic acid, and the rest is water. The polyvinyl alcohol or polyacrylic acid is uniformly distributed in the solvent.

2. The activation solution for the SCR denitration catalytic module according to claim 1, characterized in that: The solvent of the regeneration liquid is divided into two groups, A and B. The solvent of group A is used to dissolve polyacrylamide. The ammonium metavanadate, ammonium metatungstate and ammonium metamolybdate are ground to at least 10,000 mesh and put into the solvent of group B to form a suspension. The suspension is evenly added to the solvent of group A for dissolving polyacrylamide, and stirring is continued until the ammonium metavanadate, ammonium metatungstate and ammonium metamolybdate are dissolved.

3. The activation solution for the SCR denitration catalytic module according to claim 2, characterized in that: After the suspension is added, an alkaline pH regulator is introduced into the system until the pH value of the system is maintained at 11-12. After the ammonium metavanadate, ammonium metatungstate and ammonium metamolybdate are completely dissolved, an acidic pH regulator is added into the system until the pH value of the system is maintained at 7-8.

4. The activation solution for the SCR denitration catalytic module according to claim 3, characterized in that: The alkaline pH regulator is ammonia water, and the acidic pH regulator is an organic acid.

5. The activation solution for the SCR denitration catalytic module according to claim 2, characterized in that: The mass ratio of polyacrylamide to the solvent of group A is not greater than 0.5wt%.

6. The activation solution for the SCR denitration catalytic module according to any one of claims 1 to 5, characterized in that: The regeneration liquid also includes 0.2-0.7 wt % of polyethylene glycol octyl ether and 1-1.2 wt % of cetylpyridinium bromide.

7. An activation method for an SCR denitration catalytic module, characterized in that: S1: Mechanically clean the pores of the deactivated SCR denitration catalytic module; S2: The adsorption liquid is evenly coated on the surface of the cleaned SCR denitration catalytic module pores by spraying or soaking; S3: uniformly coating the regeneration liquid on the pore surface of the SCR denitration catalytic module treated in step S2 by spraying or soaking; S4: calcining the SCR denitration catalytic module treated in step S3 at 600-700° C. for 1.5-2.5 hours.

8. The method for activating the SCR denitration catalytic module according to claim 8, characterized in that: In step S2, the impregnated SCR denitration catalytic module is dried at 80-90°C for 0.5-1h.

9. The method for activating the SCR denitration catalytic module according to claim 8 or 9, characterized in that: Repeat steps S2-S4 according to the content of active components in the SCR denitration catalyst module.