Preparation process of urea solution for vehicles

Through the mixing of modified hydrotalcite and urea and the addition of antifreeze, combined with the co-precipitation method of modified Fe3O4 nanoparticles and chitosan, the adsorption problem of impurities in the urea solution is solved, and the purity of the urea solution and the NOx reduction efficiency are improved. , suitable for mass production and reduces costs.

CN119056246APending Publication Date: 2024-12-03ANHUI SOBLUE ENVIRONMENT PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411335594.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the urea solution still produces partial biuret and triuret during purification, which affects the purity and reaction rate of urea. The urea produced by traditional urea formulas is not purified enough, resulting in a reduced catalytic reduction efficiency.

Method used

Modified hydrotalcite is mixed with urea and added with antifreeze. Modified hydrotalcite is prepared by co-precipitation method of modified Fe3O4 nanoparticles and chitosan, which improves the specific surface area and magnetic properties of hydrotalcite, and effectively adsorbs impurities in water. Salt and metal ions form a high purity urea solution.

Benefits of technology

It effectively removes impurities in water, improves the purity of urea solution and NOx reduction efficiency, is suitable for large-scale production, reduces economic costs, and improves catalytic reduction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005058153560000081
    Figure BDA0005058153560000081
  • Figure BDA0005058153560000091
    Figure BDA0005058153560000091
Patent Text Reader

Abstract

The invention discloses a preparation process of an automotive urea solution, and belongs to the technical field of automobile exhaust treatment solutions, the preparation process comprises the following steps: S1, adding modified hydrotalcite into water, stirring, and filtering; s2, heating the filtered water to 30-35 DEG C, adding urea, stirring, and cooling to obtain a mixed solution; and S3, adding an anti-freezing agent into the mixed solution, and uniformly stirring to obtain the urea solution for vehicles. According to the preparation process of the urea solution for the vehicle, firstly, water is added into the modified hydrotalcite for filtering, phosphate, metal ions and the like in the water can be effectively and specifically adsorbed and removed, the adopted modified hydrotalcite is high in adsorption efficiency and easy to separate, a high-purity aqueous solution is finally obtained, then the aqueous solution is mixed with the urea, and the high-purity aqueous solution is obtained. And finally, adding the anti-freezing agent and uniformly mixing to obtain the high-purity vehicle urea solution with a good anti-freezing effect, the application range is wide, the process is simple, the economic cost is low, and the method is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of automobile exhaust treatment solutions, and in particular relates to a preparation process of a vehicle urea solution. Background Art

[0002] As the number of cars in my country continues to increase, the harm of nitrogen oxides and particulate matter emitted by cars to human health and the atmospheric environment has attracted great attention. It is reported that countries around the world are committed to reducing these two emissions. As far as my country is concerned, the "National IV" emission standard that has been implemented means that more advanced technology must be used to reduce the emission of automobile exhaust.

[0003] A large number of experimental studies have shown that selective catalytic reduction technology (SCR) is the most suitable "National IV" emission solution for diesel vehicles. This technology must use urea solution to reduce NO in exhaust gas. x Urea SCR technology injects a certain amount of urea solution into the exhaust pipe, and then the urea is evaporated, pyrolyzed and hydrolyzed to obtain the reducing agent NH3. NH3 selectively converts NO into x Reduction to N2, thereby reducing NO x emissions.

[0004] Diesel vehicles have high requirements for the purity and cleanliness of urea solution for vehicles. During the production and packaging process of urea, metal ions (sodium, magnesium, potassium, calcium, iron, zinc, chromium, etc.) and urea condense into impurities such as biuret and melamine at high temperature. The impurities phosphorus, phosphate and metal ions (sodium, magnesium, potassium, calcium, iron, zinc, chromium, etc.) present in the aqueous solution affect the activity of the SCR catalyst, and then affect the catalytic reduction efficiency. In the prior art, three-stage urea crystallization and purification are carried out to address this problem, but some biuret and triuret are still produced during the purification process. Therefore, reducing the production of biuret and triuret and increasing the solubility of urea are problems that need to be solved in this field. In traditional urea formulas, the processed urea is often not pure enough. At the same time, no improver is added during the preparation of urea solution, and the slow reaction of urea easily leads to problems such as reduced reaction rate. Summary of the invention

[0005] The object of the present invention is to provide a process for preparing a vehicle urea solution to solve one of the problems mentioned in the background technology.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A process for preparing a vehicle urea solution comprises the following steps:

[0008] Step S1, adding the modified hydrotalcite into water, stirring, and filtering;

[0009] Step S2, heating the filtered water to 30-35° C., adding urea, stirring, and cooling to obtain a mixed solution;

[0010] Step S3: adding antifreeze to the mixed solution and stirring until it is uniform to obtain a vehicle urea solution.

[0011] In some embodiments of the present invention, the weight ratio of the modified hydrotalcite to water in step S1 is 15-20:80-100.

[0012] In some embodiments of the present invention, the modified hydrotalcite is prepared by the following steps:

[0013] Chitosan and modified Fe3O4 nanoparticles were added to acetic acid solution, stirred for 2-3 hours, hydrotalcite was added, the temperature was raised to 60-65°C, formaldehyde was added and the reaction was continued with stirring for 1 hour, the pH was adjusted to 8.8-9.0, glutaraldehyde was added, stirred for 3-4 hours, filtered and collected, washed until the pH was neutral, and dried to constant weight to obtain modified hydrotalcite.

[0014] In some embodiments of the present invention, the usage ratio of chitosan and modified Fe3O4 nanoparticles, acetic acid solution, hydrotalcite, formaldehyde and glutaraldehyde is 0.48-0.50 g: 0.48-0.50 g: 150 mL: 0.12-0.15 g: 8 mL: 12 mL.

[0015] In some embodiments of the present invention, the weight ratio of the filtered water to urea in step S2 is 62-65:31-34.

[0016] In some embodiments of the present invention, the antifreeze agent includes one of methanol, ethanol, and ethylene glycol.

[0017] In some embodiments of the present invention, the amount of the antifreeze agent is 20%-25% by weight of the urea.

[0018] In some embodiments of the present invention, the modified Fe3O4 nanoparticles are prepared by the following steps:

[0019] Add FeSO4·7H2O and FeCl3·6H2O to deionized water, stir under nitrogen atmosphere, heat to 60-65°C, add ammonia water and continue stirring to react for 0.5-1h, add epichlorohydrin, heat to 70-75°C and keep stirring for 1-2h, cool to room temperature, collect Fe3O4, wash until the supernatant is neutral, centrifuge, vacuum dry, and grind to obtain modified Fe3O4 nanoparticles.

[0020] In some embodiments of the present invention, the usage ratio of FeSO4·7H2O, FeCl3·6H2O, deionized water, ammonia water and epichlorohydrin is 0.023-0.025 mol: 0.046-0.048 mol: 150 mL: 20 mL: 3.0-3.5 mL.

[0021] Beneficial effects of the present invention:

[0022] The invention discloses a process for preparing a urea solution for a vehicle. First, water is added to the modified hydrotalcite for filtering, so that phosphates and metal ions in the water can be effectively and specifically adsorbed and removed. The modified hydrotalcite has high adsorption efficiency and is easy to separate, and finally a high-purity aqueous solution is obtained. The aqueous solution is then mixed with urea, and finally an antifreeze agent is added and mixed evenly to obtain a high-purity urea solution for a vehicle with good antifreeze effect, thereby improving NO x The reduction efficiency is high, the application range is wide, and the preparation process is simple, economical, and suitable for large-scale production.

[0023] In the present invention, water is adsorbed by modified hydrotalcite. Hydrotalcite has a strong adsorption capacity due to its high specific surface area and porous structure. In the above technical scheme, chitosan, modified Fe3O4 nanoparticles and hydrotalcite are reacted and mixed by coprecipitation method. After the modified Fe3O4 nanoparticles and chitosan undergo cross-linking reaction, they are loaded on the interlayer and surface of hydrotalcite to obtain modified hydrotalcite. On the one hand, the specific surface area, porosity and dispersibility of hydrotalcite are increased, and the adsorption of impurities such as phosphorus and phosphate in aqueous solution is improved. On the other hand, the magnetic properties of hydrotalcite are given, so that the modified hydrotalcite dispersed in water can be quickly separated from the aqueous solution under the action of an external magnetic field, further improving the solid-liquid separation efficiency and recycling efficiency of hydrotalcite. In addition, the chitosan molecular structure coated on its surface has a large number of amino groups and hydroxyl groups, ether bonds and acetylamino groups, which further enhances the adsorption rate of phosphate. The introduction of modified Fe3O4 nanoparticles not only enhances the electrostatic interaction between chitosan and phosphate, thereby efficiently removing phosphate, but also overcomes the problems of poor stability, small specific surface area and poor mechanical strength of chitosan. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The modified Fe3O4 nanoparticles used in the examples and comparative examples of the present invention are prepared by the following steps:

[0026] 0.023 mol of FeSO4·7H2O and 0.046 mol of FeCl3·6H2O were added to 150 mL of deionized water, stirred under a nitrogen atmosphere, heated to 60°C, 20 mL of ammonia water (25 wt%) was added and the reaction was continued with stirring for 0.5 h, 3 mL of epichlorohydrin was added to the solution, heated to 75°C and kept stirring for 1 h, cooled to room temperature, and the black magnetic Fe3O4 was collected with a magnet. It was repeatedly washed with deionized water and ethanol until the supernatant was neutral, the solid phase material was separated by centrifugation, placed in a vacuum drying oven at 60°C and dried for 24 h, and Fe3O4 nanoparticles were obtained after grinding.

[0027] Example 1

[0028] This embodiment provides a modified hydrotalcite, and the preparation steps are as follows:

[0029] Add 0.48g chitosan and 0.48g modified Fe3O4 nanoparticles to 150mL acetic acid solution (2wt%), stir for 2h, add 0.125g hydrotalcite, heat to 60°C, add 8mL formaldehyde and continue stirring to react for 1h, adjust the pH to 8.8, add 12mL glutaraldehyde, stir for 3-4h, collect by filtration, wash until the pH is neutral, and finally dry in a 60°C oven to constant weight to obtain modified hydrotalcite.

[0030] Example 2

[0031] This embodiment provides a modified hydrotalcite, and the preparation steps are as follows:

[0032] 0.48 g of chitosan and 0.50 g of modified Fe3O4 nanoparticles were added to 150 mL of acetic acid solution (2 wt%), stirred for 2 h, 0.15 g of hydrotalcite was added, the temperature was raised to 60 ° C, 8 mL of formaldehyde was added and the reaction was continued with stirring for 1 h, the pH was adjusted to 8.8, and 12 mL of glutaraldehyde was added, stirred for 3 h, filtered and collected, washed until the pH was neutral, and finally placed in a 60 ° C oven to dry to constant weight to obtain modified hydrotalcite.

[0033] Example 3

[0034] This embodiment provides a process for preparing a vehicle urea solution, comprising the following steps:

[0035] Step S1, weighing by weight, adding 15 parts of the modified hydrotalcite in Example 1 to 80 parts of water, stirring, and filtering;

[0036] Step S2, weighing by weight, heating 62 parts of filtered water to 30° C., adding 31 parts of urea, stirring, and cooling to obtain a mixed solution;

[0037] Step S3, adding methanol to the mixed solution in an amount of 20% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0038] Example 4

[0039] This embodiment provides a process for preparing a vehicle urea solution, comprising the following steps:

[0040] Step S1, weighing by weight, adding 15 parts of the modified hydrotalcite in Example 2 to 80 parts of water, stirring, and filtering;

[0041] Step S2, weighing by weight, heating 62 parts of filtered water to 30° C., adding 31 parts of urea, stirring, and cooling to obtain a mixed solution;

[0042] Step S3, adding methanol to the mixed solution in an amount of 20% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0043] Example 5

[0044] This embodiment provides a process for preparing a vehicle urea solution, comprising the following steps:

[0045] Step S1, weighing by weight, adding 20 parts of the modified hydrotalcite in Example 1 to 100 parts of water, stirring, and filtering;

[0046] Step S2, weighing by weight, heating 65 parts of filtered water to 30° C., adding 34 parts of urea, stirring, and cooling to obtain a mixed solution;

[0047] Step S3, adding methanol to the mixed solution in an amount of 25% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0048] Example 6

[0049] This embodiment provides a process for preparing a vehicle urea solution, comprising the following steps:

[0050] Step S1, weighing by weight, adding 18 parts of the modified hydrotalcite in Example 1 to 80 parts of water, stirring, and filtering;

[0051] Step S2, weighing by weight, heating 62 parts of filtered water to 30° C., adding 32 parts of urea, stirring, and cooling to obtain a mixed solution;

[0052] Step S3, adding ethylene glycol to the mixed solution in an amount of 22% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0053] Example 7

[0054] This embodiment provides a process for preparing a vehicle urea solution, comprising the following steps:

[0055] Step S1, weighing by weight, adding 18 parts of the modified hydrotalcite in Example 1 to 95 parts of water, stirring, and filtering;

[0056] Step S2, weighing by weight, heating 64 parts of filtered water to 35° C., adding 34 parts of urea, stirring, and cooling to obtain a mixed solution;

[0057] Step S3, adding ethylene glycol to the mixed solution in an amount of 20% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0058] Comparative Example 1

[0059] This comparative example provides a preparation process of a vehicle urea solution, comprising the following steps:

[0060] Step S1, weigh by weight, add 15 parts of hydrotalcite to 80 parts of water, stir, and filter;

[0061] Step S2, weighing by weight, heating 62 parts of filtered water to 30° C., adding 31 parts of urea, stirring, and cooling to obtain a mixed solution;

[0062] Step S3, adding methanol to the mixed solution in an amount of 20% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0063] Comparative Example 2

[0064] This comparative example provides a preparation process of a vehicle urea solution, comprising the following steps:

[0065] Step S1, weighing by weight, adding 10 parts of the modified hydrotalcite in Example 1 to 80 parts of water, stirring, and filtering;

[0066] Step S2, weighing by weight, heating 62 parts of filtered water to 30° C., adding 31 parts of urea, stirring, and cooling to obtain a mixed solution;

[0067] Step S3, adding methanol to the mixed solution in an amount of 20% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0068] Comparative Example 3

[0069] This comparative example provides a preparation process of a vehicle urea solution, comprising the following steps:

[0070] Step S1, weighing by weight, adding 30 parts of the modified hydrotalcite in Example 1 to 80 parts of water, stirring, and filtering;

[0071] Step S2, weighing by weight, heating 62 parts of filtered water to 30° C., adding 31 parts of urea, stirring, and cooling to obtain a mixed solution;

[0072] Step S3, adding methanol to the mixed solution in an amount of 20% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0073] Comparative Example 4

[0074] This comparative example provides a preparation process of a vehicle urea solution, comprising the following steps:

[0075] Step S1, weighing by weight, adding 15 parts of the modified hydrotalcite in Example 1 to 80 parts of water, stirring, and filtering;

[0076] Step S2, weighing by weight, heating 62 parts of filtered water to 30° C., adding 27 parts of urea, stirring, and cooling to obtain a mixed solution;

[0077] Step S3, adding methanol to the mixed solution in an amount of 20% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0078] Comparative Example 5

[0079] This comparative example provides a preparation process of a vehicle urea solution, comprising the following steps:

[0080] Step S1, weighing by weight, adding 15 parts of the modified hydrotalcite in Example 1 to 80 parts of water, stirring, and filtering;

[0081] Step S2, weighing by weight, heating 62 parts of filtered water to 30° C., adding 38 parts of urea, stirring, and cooling to obtain a mixed solution;

[0082] Step S3, adding methanol to the mixed solution in an amount of 20% of the weight of urea, stirring until uniform, to obtain a vehicle urea solution.

[0083] The automotive urea obtained in Examples 3 to 7 and Comparative Examples 1 to 5 was tested, and the test results are shown in Table 1:

[0084] Table 1

[0085]

[0086]

[0087] It can be seen from Table 1 that the biuret purity, alkalinity, aldehyde substances, insoluble matter and phosphate content of the automotive urea solutions prepared in Examples 3-7 are all lower than those in Comparative Examples 1-5, and a urea solution with higher purity is obtained, which has greater application value.

[0088] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0089] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for preparing a urea solution for a vehicle, characterized in that: The following steps are involved: Step S1, adding the modified hydrotalcite into water, stirring, and filtering; Step S2, heating the filtered water to 30-35° C., adding urea, stirring, and cooling to obtain a mixed solution; Step S3: adding antifreeze to the mixed solution and stirring until it is uniform to obtain a vehicle urea solution.

2. The process for preparing a vehicle urea solution according to claim 1, characterized in that: In step S1, the weight ratio of the modified hydrotalcite to water is 15-20:80-100.

3. The process for preparing a vehicle urea solution according to claim 1, characterized in that: The modified hydrotalcite is prepared by the following steps: Chitosan and modified Fe3O4 nanoparticles were added to acetic acid solution, stirred for 2-3 hours, hydrotalcite was added, the temperature was raised to 60-65°C, formaldehyde was added and the reaction was continued with stirring for 1 hour, the pH was adjusted to 8.8-9.0, glutaraldehyde was added, stirred for 3-4 hours, filtered and collected, washed until the pH was neutral, and dried to constant weight to obtain modified hydrotalcite.

4. The process for preparing a urea solution for vehicle according to claim 3, characterized in that: The dosage ratio of chitosan, modified Fe3O4 nanoparticles, acetic acid solution, hydrotalcite, formaldehyde and glutaraldehyde is 0.48-0.50g: 0.48-0.50g: 150mL: 0.12-0.15g: 8mL: 12mL.

5. The process for preparing a vehicle urea solution according to claim 1, characterized in that: The weight ratio of the filtered water to urea in step S2 is 62-65:31-34.

6. The process for preparing a vehicle urea solution according to claim 1, characterized in that: The antifreeze agent includes one of methanol, ethanol and ethylene glycol.

7. The process for preparing a vehicle urea solution according to claim 1, characterized in that: The dosage of the antifreeze agent is 20%-25% of the weight of urea.

8. The process for preparing a vehicle urea solution according to claim 1, characterized in that: The modified Fe3O4 nanoparticles are prepared by the following steps: Add FeSO4·7H2O and FeCl3·6H2O to deionized water, stir under nitrogen atmosphere, heat to 60-65°C, add ammonia water and continue stirring to react for 0.5-1h, add epichlorohydrin, heat to 70-75°C and keep stirring for 1-2h, cool to room temperature, collect Fe3O4, wash until the supernatant is neutral, centrifuge, vacuum dry, and grind to obtain modified Fe3O4 nanoparticles.

9. The process for preparing a vehicle urea solution according to claim 8, characterized in that: The dosage ratio of FeSO4·7H2O, FeCl3·6H2O, deionized water, ammonia water and epichlorohydrin is 0.023-0.025 mol: 0.046-0.048 mol: 150 mL: 20 mL: 3.0-3.5 mL.