High-crystallinity PVDF (Polyvinylidene Fluoride) ultrafiltration membrane for treating mining wastewater and preparation method of high-crystallinity PVDF ultrafiltration membrane
By introducing ultra-high molecular weight comb polymer and induced crystallization technology into PVDF ultrafiltration membrane, a high-crystalline film that is resistant to friction and scratches is formed, which solves the problem of membrane damage in mining wastewater treatment and achieves long-term and stable operation of the membrane and efficient separation effect.
Patent Information
- Application Number
- CN202411304220.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
AI Technical Summary
When treating mining wastewater, the existing PVDF ultrafiltration membrane has a short film service life due to frictional damage between fine ore sand particles and heavy metal particles. The existing enhancement process fails to effectively improve the friction and scratch resistance of the membrane, which limits the Its application in mining wastewater treatment.
UHM-weight comb polymer is blended with PVDF, and through grafting reaction and induction crystallization technology, a high crystallinity film surface with strong intermolecular cohesion is formed, improving the film's friction and scratch resistance.
The prepared high-crystalline PVDF ultrafiltration membrane is not prone to damage when treating mining wastewater, maintains stable operation, and has a simple process and is suitable for industrial production.
Smart Images

Figure CN119056273A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment ultrafiltration membranes, and specifically relates to a high-crystallinity PVDF ultrafiltration membrane for treating mining wastewater and a preparation method thereof. Background Art
[0002] The rapid economic development requires a large amount of raw materials. As an important resource, minerals are increasingly mined, which leads to serious water pollution problems. In the process of mining, a large amount of rainwater will collect in the mine when it rains. This rainwater will wash the surface of the mine and carry away the ore particles to form rainwater containing pollutants. Whether it is open-pit mining or underground mining, there is groundwater deep in the mine that needs to be discharged continuously to ensure the safety and normal operation of mining operations. After contacting with the ore, these groundwaters carry away minerals and heavy metals in the ore, forming groundwater containing pollutants. In the process of ore processing and transportation, in order to reduce dust flying, water is usually sprayed to reduce dust. These waters are mixed with ore powder and become wastewater containing pollutants. In the process of mineral gravity separation and magnetic separation, in order to effectively separate the ore particles in the equipment, water is needed to wash the ore, and these waters eventually become wastewater containing pollutants. The polluted water produced above is collectively called mining wastewater. Compared with ordinary domestic sewage, mining wastewater contains a large amount of mineral components, mainly some fine mineral sand particles and heavy metal particles. These substances are biologically toxic and cannot be naturally degraded. Therefore, mining wastewater must be strictly treated to avoid polluting the environment.
[0003] In the treatment of mining wastewater, the use of ultrafiltration membrane filtration has become an increasingly important means. Ultrafiltration membranes can not only completely remove pollutants visible to the naked eye in the water, but also remove most of the pollutants invisible to the naked eye. Mining wastewater treated by ultrafiltration membranes can meet the discharge standards or be reused. At present, most of the ultrafiltration membranes used in mining wastewater treatment are made of inorganic materials (such as alumina, silicon dioxide, silicon carbide, etc.) or PTFE materials. The membranes made of these materials are resistant to acid and alkali, corrosion, and high temperature, have high mechanical strength, are not easy to damage, and have a long service life. However, the interception accuracy is not high, the processing is difficult, the manufacturing cost is high, and the maintenance cost is also high, which limits the large-scale application of membrane technology in mining wastewater.
[0004] PVDF (polyvinylidene fluoride) has become one of the ideal materials for preparing ultrafiltration membranes due to its good film-forming properties and excellent physical and chemical stability. The process of using PVDF materials to prepare ultrafiltration membranes is simple and low-cost, and the membrane has a high retention rate, good separation effect, and is easy to maintain and clean. PVDF ultrafiltration membranes have been widely used in water plant renovation, domestic sewage treatment, seawater desalination pretreatment and other fields. However, in the field of mining wastewater treatment, PVDF ultrafiltration membranes are not widely used. The reason is that the surface of tiny mineral sand particles and heavy metal particles in the wastewater is as sharp as a knife edge. When they rub against the PVDF ultrafiltration membrane in water, the outer surface cortex of the membrane is damaged, resulting in a decrease in the separation effect and a serious reduction in the service life of the membrane. In order to increase the physical strength of PVDF ultrafiltration membrane, many processes have been developed, and a large number of studies and methods have been reported: Patent CN102430348B discloses a method for preparing a polyester braided tube / polymer composite hollow fiber membrane, Patent CN102512990B discloses a method for preparing an internally supported polyvinylidene fluoride hollow fiber membrane, and Patent 102784566B discloses a method for preparing a heterogeneously reinforced polyvinylidene fluoride hollow fiber membrane with high burst strength. Most of these methods use chemical and physical methods to strengthen the bonding force between the membrane layer and the supporting layer material, so that the membrane is not easy to peel off, resistant to recoil, and resistant to mechanical vibration, but it has no obvious effect on strengthening the strength of the outermost cortex of the membrane in direct contact with pollutants, and there is no literature report on strengthening the friction resistance and scratch resistance of the membrane and improving the service life of the membrane in mining wastewater treatment. Therefore, it is of great academic significance and economic value to find a simple and easy-to-industrial method to prepare a PVDF ultrafiltration membrane that can operate stably for a long time in mining wastewater and has a high-strength outer surface. Summary of the invention
[0005] The purpose of the present invention is to provide a high-crystallinity PVDF ultrafiltration membrane for treating mining wastewater and a preparation method thereof. The method is simple, the process is stable and reliable, and is suitable for industrial production. The prepared PVDF ultrafiltration membrane has an outer surface formed by crystals formed by PVDF wrapped around an ultra-high molecular weight comb-like polymer. The crystals have strong intermolecular cohesion, and the membrane surface formed by them is resistant to friction and scratching. When treating mining wastewater containing a large amount of fine mineral sand particles and heavy metal particles, the membrane layer is not easily damaged and can maintain stable operation.
[0006] To achieve the above object, the present invention provides a method for preparing a high-crystallinity PVDF ultrafiltration membrane for treating mining wastewater, comprising the following steps: S1, synthesis of ultra-high molecular weight comb polymer; Add an acrylic copolymer to anhydrous DMSO solvent and dissolve it evenly, then add hydroxyl-terminated polyester under stirring and mix evenly until transparent, then add a crosslinking agent under stirring and heat to reaction temperature to start grafting reaction, stop heating and stirring after a period of reaction, and cool to room temperature to obtain an ultra-high molecular weight comb polymer solution; S2, preparing a PVDF ultrafiltration membrane casting solution containing an ultrahigh molecular weight comb-like polymer; Add the solution containing the ultrahigh molecular weight comb-like polymer prepared in step S1 to the solvent DMAC, and add a small amount of surfactant and small molecule salt, stir to make them uniformly dispersed in DMAC, then add PVDF under stirring, heat to 75° C. to dissolve evenly, finally add a certain amount of porogen, stir for a period of time, stop stirring, stand and degas to obtain a PVDF ultrafiltration membrane casting solution containing the ultrahigh molecular weight comb-like polymer; S3, preparing high crystallinity PVDF ultrafiltration membrane; The casting liquid prepared in step S2 is made into a liquid film through a spinning device or a scraping device, and then cooled and solidified in a non-solvent phase containing an inducer, and a solid film is formed through a solution phase conversion process. The solvent in the film is cleaned with clean water, and finally naturally dried to obtain a high-crystallinity PVDF ultrafiltration membrane.
[0007] Preferably, in step S1, the mass percentages of the acrylic copolymer, the crosslinking agent, and the hydroxyl-terminated polyester in the solvent are 8-10%, 0.2-0.2%, and 2-4%, respectively.
[0008] Preferably, in step S1, the reaction temperature is 80-85°C; the reaction time is 2-4h; and the heating rate is 1-2°C / min.
[0009] Preferably, in step S1, the acrylic copolymer is PARALOID™ BPMS-250 or PARALOID™ BPMS-260.
[0010] Preferably, in step S1, the hydroxyl-terminated polyester is polypropylene carbonate (PPC); and the cross-linking agent is isophorone diisocyanate (IPDI) or hexamethylene diisocyanate (HDI).
[0011] Preferably, in step S2, the mass percentages of the ultra-high molecular weight comb polymer solution, surfactant, small molecule salt, PVDF, and porogen in the solvent DMAC are: 45-55%, 0.1-0.2%, 1-2%, 24-26%, and 4-6%, respectively.
[0012] Preferably, in step S2, the surfactant is octadecyl ammonium chloride (STAC) or hexadecyl ammonium chloride (CTAC); the small molecule salt is lithium nitrate or calcium nitrate; and the porogen is polyvinyl pyrrolidone (PVP) or polyethylene glycol (PEG).
[0013] Preferably, in step S3, the non-solvent phase is a mixture of water and alcohol, the volume fraction of alcohol to water is 30%-40%, and the temperature of the non-solvent phase is -15°C to -5°C.
[0014] Preferably, in step S3, the inducer is sodium silicate, and the content of the inducer in the non-solvent phase is 1%-2%.
[0015] To achieve the above object, the present invention provides a high-crystallinity PVDF ultrafiltration membrane for treating mining wastewater prepared by the above preparation method, wherein the PVDF ultrafiltration membrane includes two forms: a hollow ultrafiltration membrane and a flat ultrafiltration membrane.
[0016] like Figure 1 As shown, the present invention first prepares an ultra-high molecular weight comb-like polymer, which is a polymer with a special structure, mainly composed of a main chain and a side chain. The main chain is the main skeleton of the polymer, and the side chains are arranged at both ends of the main chain like the teeth of a comb. There is only one main chain and many side chains, forming a comb-like structural appearance. When the polymer with a comb-like structure is blended with PVDF to form a film, the densely arranged side chains at both ends are easy to cross-entangle with PVDF to form a network structure. The molecular clusters formed by this network structure greatly enhance the intermolecular force. The casting liquid formed by blending the ultra-high molecular weight comb-like polymer with PVDF and other additives is transformed into a liquid film of a certain form through a film-making device. The liquid film is rapidly crystallized under the combined action of cooling and an inducing agent, and solidified into a film in a non-solvent phase. The surface of the formed ultrafiltration membrane is composed of a large number of crystals, and the molecules have a strong internal cohesion, so the outer surface is resistant to friction and scratches.
[0017] In the present invention, an acrylate copolymer PARALOID™ BPMS-250 and PARALOID™ BPMS-260 are used. The material is produced by Dow Chemical and is a copolymer formed by polymerization of three monomers: methyl acrylate (MA), butyl acrylate (BA), and hydroxyethyl acrylate (HEA). The molecular formula can be expressed as: P-[-(MA)x-(BA)y-(HEA)z-]-. It has a main chain connected by ultra-long carbon atoms, and the side chain is a large number of saturated fatty acid esters. The molecular weight is very high, all above one million. At present, the material is used as a melt enhancer. In some polymer melt processing processes, a certain proportion of the material is added, and the ultra-long side chains with high relative molecular mass can be cross-entangled with low relative molecular mass polymer plastics or resins to form a network structure in the molten state, thereby improving the strength of the melt. In the present invention, it is used as a starting reactant because the material has a very high molecular weight, and the prepared comb-like polymer molecular weight will be higher. In addition, the material has good reactivity, and the side chain has a large number of ester groups that are easy to graft.
[0018] The technical difficulties of the present invention mainly include two points: one is the uniform dispersion and stable existence of the comb-like polymer in the casting liquid, and the other is that the liquid film forms stable and effective crystals during the solidification process. The molecular weight of the synthesized comb-like polymer is very high and there is an interaction force between the molecules, so it is not easy to disperse and dissolve in DMAC. Therefore, it is necessary to add some small molecule salts to destroy the interaction between the comb-like polymer and the comb-like polymer to improve its solubility; in order to prevent the dispersed comb-like polymer from reaggregating during the film-making process, it is necessary to add some surfactants. The surfactant provides a certain charge repulsion around the comb-like polymer, which can make the dispersed and dissolved ultra-high molecular weight comb polymer stable. The addition of these surfactants cannot affect the film-making. In order to make the liquid film form stable and effective crystals during the solidification process, the crystallization rate of the molecular clusters formed by the comb-like polymer and PVDF must be accelerated, so the inducer to be added in the non-solvent phase and low-temperature cooling is adopted. In the present invention, Na is selected 2 SiO 3 As an inducer, this is because Na 2 SiO 3 In the water, they are tiny crystal nuclei. When they encounter other easily crystallized substances, they will crystallize quickly. Low-temperature cooling is required. Because pure water cannot reach temperatures below zero, a mixture of pure water and alcohol is used as the non-solvent phase.
[0019] Compared with the prior art, the present invention has the following advantages: The PVDF ultrafiltration membrane prepared by the present invention has a crystal formed by PVDF wrapped around an ultrahigh molecular weight comb-shaped polymer on its outer surface. The crystal has a strong intermolecular cohesion, and the membrane surface formed by it is resistant to friction and scratches. When treating mining wastewater containing a large amount of fine ore sand particles and heavy metal particles, the membrane layer is not easily damaged and can maintain stable operation. The method is simple to operate, the process is stable and reliable, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic diagram of the principle of the present invention; Figure 2 This is a surface electron micrograph of the high crystallinity PVDF ultrafiltration membrane prepared in Example 1; Figure 3 This is a surface electron microscope image of the PVDF ultrafiltration membrane prepared in Comparative Example 1. DETAILED DESCRIPTION
[0021] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments. Example
[0022] A method for preparing a high-crystallinity PVDF ultrafiltration membrane for treating mining wastewater comprises the following steps: S1, synthesis of ultra-high molecular weight comb polymer; 10 g of PARALOID™ BPMS-250 produced by Dow Chemical was added to 100 g of anhydrous DMSO and dissolved uniformly, and then 4 g of PPC was added under stirring to mix into a uniform transparent solution, and then 0.3 g of IPDI was added under stirring and the temperature was rapidly increased to 85°C at a heating rate of 1°C / min to start the reaction. After reacting for 4 hours, heating and stirring were stopped, and the mixture was cooled to room temperature to obtain an ultra-high molecular weight comb polymer solution. The molecular weight of the comb polymer was between 2.8 million and 3.2 million Daltons as determined by GPC. S2, preparing a PVDF ultrafiltration membrane casting solution containing an ultrahigh molecular weight comb-like polymer; 45 g of ultra-high molecular weight comb polymer solution was added to 100 g of DMAC, and 0.1 g of STAC and 1 g of LiNO were added. 3 , stir evenly to form a transparent solution, then add 24g PVDF under stirring, heat to 75°C to dissolve evenly, finally add 4g PVP to dissolve and stir evenly, stop stirring, let stand and degas to obtain a PVDF ultrafiltration membrane casting solution containing ultrahigh molecular weight comb-like polymer; S3, preparing high crystallinity PVDF ultrafiltration membrane; The PVDF ultrafiltration membrane casting solution containing ultrahigh molecular weight comb polymer was made into a flat liquid membrane on a scraped membrane device, and then heated at -5℃ and containing 2% Na 2 SiO3 The membrane is cooled and solidified in a mixture of water and alcohol (the volume fraction of alcohol in water is 30%), and a solid membrane is formed through a solution phase conversion process. The solvent in the membrane is then washed away with clean water, and finally dried naturally to obtain a PVDF flat ultrafiltration membrane with high crystallinity.
[0023] The flat ultrafiltration membrane prepared in this example was tested and the performance was as follows: the pure water flux at 20°C under a pressure of 0.1 MPa was 1250 L / m 2 h, average pore size is 90 nm, pure water bubble point is 0.12 MPa, from Figure 2 A large number of crystals can be clearly seen in the figure. The prepared flat ultrafiltration membrane was placed in 1 L of pure water, and then 50g of quartz sand and 10g of lead powder were added to the water, and then it was shaken continuously. After a certain shaking time, the pure water flux and bubble point were measured. The results are shown in Table 1 below. It can be seen that the flux and bubble point did not change much, indicating that the performance of this ultrafiltration membrane was stable in water with fine mineral sand particles and heavy metal particles.
[0024] Table 1 Performance test results of the flat ultrafiltration membrane prepared in this example Oscillation time (days) 0 1 2 3 4 Flux (LMH) 1250 1260 1300 1280 1280 Bubble point (MPa) 0.12 0.12 0.12 0.12 0.12 Comparative Example 1 The difference from Example 1 is that no ultra-high molecular weight comb polymer is added to the casting solution. The other operations are the same as follows: 0.1 g STAC and 1 g LiNO are added to 100 g DMAC. 3 , stir evenly to form a transparent solution, then add 24g PVDF, heat to 75℃ to dissolve evenly, finally add 4g PVP to dissolve and stir evenly, stop stirring, let stand to degas, and obtain PVDF ultrafiltration membrane casting solution; the casting solution is made into a flat liquid membrane on a scraping device, and then at -5℃ and containing 2% Na 2 SiO 3 The membrane is cooled and solidified in a mixture of water and alcohol (the volume fraction of alcohol in water is 30%), and a solid membrane is formed through a solution phase conversion process. The solvent in the membrane is then washed away with clean water, and finally naturally dried to obtain a PVDF flat ultrafiltration membrane.
[0025] The flat ultrafiltration membrane prepared in Comparative Example 1 was tested, and the performance was as follows: the pure water flux at 20°C under a pressure of 0.1 MPa was 1200 L / m 2 h, average pore size 95 nm, pure water bubble point 0.13 MPa, from Figure 3It can be seen that there is no crystalline structure compared with Example 1. The prepared flat ultrafiltration membrane was placed in 1 L of pure water, and then 50g of quartz sand and 10g of lead powder were added to the water, and then it was shaken continuously. After a certain shaking time, its pure water flux and bubble point were measured. The results are shown in Table 2 below. It can be seen that its flux increases rapidly and the bubble point decreases rapidly, indicating that the ultrafiltration membrane is severely damaged in the cortex under the friction of fine mineral sand particles and heavy metal particles in water.
[0026] Table 2 Performance test results of the flat ultrafiltration membrane prepared in this comparative example Oscillation time (days) 0 1 2 3 4 Flux (LMH) 1200 1860 3500 4080 4850 Bubble point (MPa) 0.13 0.08 0.03 0.01 Less than 0.01 Example
[0027] A method for preparing a high-crystallinity PVDF ultrafiltration membrane for treating mining wastewater comprises the following steps: S1, synthesis of ultra-high molecular weight comb polymer; 8 g of PARALOID™ BPMS-260 produced by Dow Chemical was added to 100 g of anhydrous DMSO and dissolved uniformly, and then 2 g of PPC was added under stirring to mix into a uniform transparent solution, and then 0.2 g of HDI was added under stirring and the temperature was rapidly increased to 80°C at a heating rate of 1.5°C / min to start the reaction. After reacting for 2 hours, heating and stirring were stopped, and the mixture was cooled to room temperature to obtain an ultra-high molecular weight comb polymer solution. The molecular weight of the comb polymer was between 3 million and 3.5 million Daltons as determined by GPC; S2, preparing a PVDF ultrafiltration membrane casting solution containing an ultrahigh molecular weight comb-like polymer; 50 g of the comb polymer solution was added to 100 g of DMAC, and 0.15 g of CTAC and 1.5 g of Ca(NO 3 ) 2 , stir evenly to form a transparent solution, then add 25g PVDF, heat to 75℃ and dissolve evenly, finally add 5g PEG and dissolve and stir evenly, then stop stirring, let stand and degas to obtain a PVDF ultrafiltration membrane casting solution containing an ultrahigh molecular weight comb-like polymer; S3, preparing high crystallinity PVDF ultrafiltration membrane; The PVDF ultrafiltration membrane casting solution containing ultrahigh molecular weight comb polymer was made into a hollow liquid membrane on a spinning device, and then heated at -15℃ and containing 1% Na 2 SiO 3 The membrane is cooled and solidified in a mixture of water and alcohol (the volume fraction of alcohol in water is 40%), and a solid membrane is formed through a solution phase transformation process. The solvent in the membrane is then washed away with clean water, and finally dried naturally to obtain a PVDF hollow ultrafiltration membrane with high crystallinity.
[0028] The hollow ultrafiltration membrane prepared in this example was tested, and the performance was as follows: the pure water flux at 20°C under a pressure of 0.1 MPa was 1200 L / m 2 h, the average pore size is 80 nm, and the pure water bubble point is 0.14 MPa. The prepared hollow ultrafiltration membrane was placed in 1 L of pure water, and then 50g of quartz sand and 10g of lead powder were added to the water, and then it was shaken continuously. After a certain shaking time, its pure water flux and bubble point were measured. The results are shown in Table 3 below. It can be seen that its flux and bubble point did not change much, indicating that the performance of this ultrafiltration membrane was stable in water with fine mineral sand particles and heavy metal particles.
[0029] Table 3 Performance test results of the flat ultrafiltration membrane prepared in this example Oscillation time (days) 0 1 2 3 4 Flux (LMH) 1200 1220 1210 1250 1210 Bubble point (MPa) 0.14 0.14 0.14 0.14 0.14 Example
[0030] A method for preparing a high-crystallinity PVDF ultrafiltration membrane for treating mining wastewater comprises the following steps: S1, synthesis of ultra-high molecular weight comb polymer; 9 g of PARALOID™ BPMS-260 produced by Dow Chemical was added to 100 g of anhydrous DMSO and dissolved uniformly, and then 3 g of PPC was added under stirring to mix into a uniform transparent solution, and then 0.25 g of HDI was added under stirring and the temperature was rapidly increased to 83°C at a heating rate of 2°C / min to start the reaction. After reacting for 3 hours, heating and stirring were stopped, and the mixture was cooled to room temperature to obtain an ultra-high molecular weight comb polymer solution. The molecular weight of the comb polymer was between 3.5 million and 4 million Daltons as determined by GPC. S2, preparing a PVDF ultrafiltration membrane casting solution containing an ultrahigh molecular weight comb-like polymer; 55 g of the comb polymer solution was added to 100 g of DMAC, and 0.2 g of STAC and 2 g of Ca(NO 3 ) 2 , stirring evenly to form a transparent solution, then adding 26g PVDF, heating to 75°C to dissolve evenly, and finally adding 6g PEG to dissolve and stir evenly, then stopping stirring, standing and degassing to obtain a PVDF ultrafiltration membrane casting solution containing an ultrahigh molecular weight comb-like polymer; S3, preparing high crystallinity PVDF ultrafiltration membrane; The PVDF ultrafiltration membrane casting solution containing ultrahigh molecular weight comb polymer was made into a hollow liquid membrane on a spinning device, and then heated at -10℃ and containing 1.5% Na 2 SiO 3The membrane is cooled and solidified in a mixture of water and alcohol (the volume fraction of alcohol in water is 35%), and a solid membrane is formed through a solution phase transformation process. The solvent in the membrane is then washed away with clean water, and finally dried naturally to obtain a PVDF hollow ultrafiltration membrane with high crystallinity.
[0031] The hollow ultrafiltration membrane prepared in this example was tested, and the performance was as follows: the pure water flux at 20°C under a pressure of 0.1 MPa was 1300 L / m 2 h, the average pore size is 90 nm, and the pure water bubble point is 0.11MPa. The prepared hollow ultrafiltration membrane was placed in 1 L of pure water, and then 50g of quartz sand and 10g of lead powder were added to the water, and then it was shaken continuously. After a certain shaking time, the pure water flux and bubble point were measured. The results are shown in Table 4 below. It can be seen that the flux and bubble point did not change much, indicating that the ultrafiltration membrane has stable performance in water with fine mineral sand particles and heavy metal particles.
[0032] Table 4 Performance test results of the flat ultrafiltration membrane prepared in this example Oscillation time (days) 0 1 2 3 4 Flux (LMH) 1300 1320 1330 1310 1310 Bubble point (MPa) 0.11 0.11 0.11 0.11 0.11 .
Claims
1. A method for preparing a high-crystallinity PVDF ultrafiltration membrane for treating mining wastewater, characterized in that: The following steps are involved: S1, synthesis of ultra-high molecular weight comb polymer; Add an acrylic copolymer to anhydrous DMSO solvent and dissolve it evenly, then add hydroxyl-terminated polyester under stirring and mix evenly until transparent, then add a crosslinking agent under stirring and heat to reaction temperature to start grafting reaction, stop heating and stirring after a period of reaction, and cool to room temperature to obtain an ultra-high molecular weight comb polymer solution; S2, preparing a PVDF ultrafiltration membrane casting solution containing an ultrahigh molecular weight comb-like polymer; Add the solution containing the ultrahigh molecular weight comb-like polymer prepared in step S1 to the solvent DMAC, and add a small amount of surfactant and small molecule salt, stir to make them uniformly dispersed in DMAC, then add PVDF under stirring, heat to 75° C. to dissolve evenly, finally add a certain amount of porogen, stir for a period of time, stop stirring, stand and degas to obtain a PVDF ultrafiltration membrane casting solution containing the ultrahigh molecular weight comb-like polymer; S3, preparing high crystallinity PVDF ultrafiltration membrane; The casting liquid prepared in step S2 is made into a liquid film through a spinning device or a scraping device, and then cooled and solidified in a non-solvent phase containing an inducer, and a solid film is formed through a solution phase conversion process. The solvent in the film is cleaned with clean water, and finally naturally dried to obtain a high-crystallinity PVDF ultrafiltration membrane.
2. The method for preparing a high crystallinity PVDF ultrafiltration membrane for treating mining wastewater according to claim 1, characterized in that: In step S1, the mass percentages of the acrylic copolymer, the crosslinking agent, and the hydroxyl-terminated polyester in the solvent are 8-10%, 0.2-0.2%, and 2-4%, respectively.
3. The method for preparing a high crystallinity PVDF ultrafiltration membrane for treating mining wastewater according to claim 1 or 2, characterized in that: In step S1, the reaction temperature is 80-85°C; the reaction time is 2-4h; and the heating rate is 1-2°C / min.
4. The method for preparing a high crystallinity PVDF ultrafiltration membrane for treating mining wastewater according to claim 1 or 2, characterized in that: In step S1, the acrylic copolymer is PARALOID™ BPMS-250 or PARALOID™ BPMS-260.
5. The method for preparing a high crystallinity PVDF ultrafiltration membrane for treating mining wastewater according to claim 1 or 2, characterized in that: In step S1, the hydroxyl-terminated polyester is polypropylene carbonate; and the cross-linking agent is isophorone diisocyanate or hexamethylene diisocyanate.
6. The method for preparing a high crystallinity PVDF ultrafiltration membrane for treating mining wastewater according to claim 1 or 2, characterized in that: In step S2, the mass percentages of the ultrahigh molecular weight comb polymer solution, the surfactant, the small molecule salt, the PVDF, and the porogen in the solvent DMAC are 45-55%, 0.1-0.2%, 1-2%, 24-26%, and 4-6%, respectively.
7. The method for preparing a high crystallinity PVDF ultrafiltration membrane for treating mining wastewater according to claim 1 or 2, characterized in that: In step S2, the surfactant is octadecyl ammonium chloride or hexadecyl ammonium chloride; the small molecule salt is lithium nitrate or calcium nitrate; and the porogen is polyvinyl pyrrolidone or polyethylene glycol.
8. The method for preparing a high crystallinity PVDF ultrafiltration membrane for treating mining wastewater according to claim 1 or 2, characterized in that: In step S3, the non-solvent phase is a mixture of water and alcohol, the volume fraction of alcohol to water is 30%-40%, and the temperature of the non-solvent phase is -15°C~-5°C.
9. The method for preparing a high crystallinity PVDF ultrafiltration membrane for treating mining wastewater according to claim 1 or 2, characterized in that: In step S3, the inducer is sodium silicate, and the content of the inducer in the non-solvent phase is 1%-2%.
10. A high-crystallinity PVDF ultrafiltration membrane for treating mining wastewater prepared by the preparation method according to any one of claims 1 to 9, wherein the PVDF ultrafiltration membrane comprises two forms: a hollow ultrafiltration membrane and a flat ultrafiltration membrane.