Novel catalyst for catalyzing and depolymerizing biomass and preparation method thereof
Through the novel catalyst preparation method, Nd2O3/NSHPC catalyst is prepared by using biomass powder and metal oxides after dilute hydrochloric acid treatment, which solves the problems of high cost and low conversion efficiency of existing catalysts, and realizes efficient lignin conversion and resource recycling , significantly improves the economical and environmental protection of catalytic dispolymerization.
Patent Information
- Application Number
- CN202411174887.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
In the directional catalytic depolymerization of existing catalysts, there are problems such as non-renewable resource, high cost and low conversion efficiency, especially the high cost and insufficient catalytic activity of precious metal and transition metal oxide catalysts.
Using a new catalyst preparation method, non-metallic catalysts are prepared by rotary evaporation, heating and impregnation using materials such as biomass powder, calcium chloride and thiourea, and treated in dilute hydrochloric acid to obtain Nd2O3/NSHPC catalysts. Catalytic disagglomeration of lignin.
It significantly reduces costs, improves the conversion rate of lignin by more than 95%, improves the economy and efficiency of the catalytic depolymerization process, and the catalyst resources are renewable, the manufacturing cost is low, the reaction conditions are mild, the generation of by-products is reduced, and the whole process is green. Environmental friendly.
Smart Images

Figure CN119056435A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and particularly relates to a novel catalyst for catalytic depolymerization of biomass and a preparation method thereof. Background Art
[0002] With the development of economy, the demand for fossil energy is increasing day by day, but fossil energy is non-renewable and its reserves are gradually decreasing, so it is urgent to find renewable energy to replace it. Biomass energy is one of the alternative energy sources. Biomass energy belongs to renewable carbon resources and has the characteristics of large output, wide source and low pollution.
[0003] In particular, lignin, a biomass component rich in benzene ring monomers, can be converted into low molecular weight aromatic compounds through targeted catalytic depolymerization technology, and is expected to replace fossil resources through biorefining, providing a new path for replacing traditional fossil resources. Among them, selective and efficient catalytic breaking of CO bonds and CC bonds is a key step in improving the utilization efficiency of lignin.
[0004] At present, the catalysts for the directed catalytic depolymerization of lignin mainly focus on precious metals, transition metals, rare earth metals and their compounds. Due to their unique properties, metals and metal oxides have shown significant advantages in reducing the conversion energy barrier and improving the efficiency and selectivity of lignin depolymerization. However, although precious metal catalysts have excellent performance, their high cost limits their widespread application; transition metal oxides face the problem of insufficient catalytic activity; at the same time, both precious metal and transition metal catalysts have problems such as non-renewable resources, high cost, and large carbon emissions during preparation and utilization. In view of this, in order to solve the problems of non-renewable resources, high cost and low lignin conversion efficiency in the preparation process of traditional catalysts, it is necessary to provide a catalytic depolymerization method based on renewable resources, low cost and significantly improving the lignin conversion rate. Summary of the invention
[0005] To achieve the above objectives, the present invention adopts the following technical solutions:
[0006] A method for preparing a novel catalyst for catalytic depolymerization of biomass comprises the following steps:
[0007] Step 1: Take some biomass, wash it, dry it, cool it to room temperature, and then grind it into biomass powder for later use;
[0008] Step 2: adding an appropriate amount of biomass powder, calcium chloride, and a first catalyst to deionized water, and stirring to obtain a mixed precursor;
[0009] Step 3: Rotate the mixed precursor to evaporate, transfer to a container after the water is completely evaporated, and dry;
[0010] Step 4: Put the dried product into a nickel crucible and place it in a tube furnace, fill it with protective gas, and heat it to obtain a crude non-metallic catalyst product;
[0011] Step 5: After the crude non-metallic catalyst product is cooled, the crude non-metallic catalyst product is immersed in dilute hydrochloric acid and continuously stirred, and then the mixed solution is filtered, and the filtered solid is washed with deionized water until the solid is neutral, and then placed in a vacuum dry to obtain a non-metallic catalyst;
[0012] Step 6: Take a corresponding mass of the second catalyst, add an appropriate amount of water to dissolve it, and obtain a second catalyst aqueous solution;
[0013] Step 7: Take an appropriate amount of the non-metallic catalyst in step 5, add it to the second catalyst aqueous solution in step 6, then add appropriate amount of water, perform ultrasonic stirring to dissolve and then immerse;
[0014] Step 8: Drying the solution impregnated in step 7;
[0015] Step nine: heat-treating the dried solution in step eight, and simultaneously injecting a protective gas for calcination, to finally obtain a new catalyst.
[0016] As a further improvement of the technical solution, the first catalyst is thiourea.
[0017] As a further improvement of the technical solution, the weight ratio of material powder: calcium chloride: catalyst is 1:2:2.
[0018] As a further improvement of the technical solution, in step four, the protective gas filled is nitrogen.
[0019] As a further improvement of the technical solution, the second catalyst is Nd(NO3)3 or Pr6O 11 .
[0020] The present application also provides a novel catalyst for catalytic depolymerization of biomass, and the catalyst is prepared by the above preparation method.
[0021] The present application also provides a method for using a novel catalyst for catalytic depolymerization of biomass, wherein lignin and the novel catalyst are added into a solvent to carry out a depolymerization reaction.
[0022] As a further improvement of the technical solution, the solvent is any one of methanol, isopropanol and ethanol.
[0023] As a further improvement of the technical solution, the solvent is methanol.
[0024] As a further improvement of the technical solution, the temperature during the depolymerization reaction is 160°C-200°C.
[0025] As a further improvement of the technical solution, the gas pressure during the depolymerization reaction is 1.5 MPa, and the pressurized gas is oxygen.
[0026] As a further improvement of the technical solution, the depolymerization reaction time is 3 hours to 5 hours.
[0027] As a further improvement of the technical solution, the depolymerization reaction time is 4 hours.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The preparation method of the present application not only significantly reduces the cost, but also has a high lignin conversion rate of more than 95%, effectively improving the economy and efficiency of the traditional depolymerization process. The reaction conditions are mild and easy to implement, effectively shortening the reaction time.
[0030] 2. The preparation method of the present application stands out in its operation process, which is easy to implement and easy to control. At the same time, the catalyst exhibits extremely high substrate conversion efficiency during the depolymerization process, ensuring the maximum utilization of raw materials. In addition, its product selectivity is excellent, and it can accurately guide the generation of target products, reduce the generation of by-products, and the green environmental protection and economic benefits of the entire depolymerization process. Various agricultural wastes, various forestry and grass industry wastes, and various crop processing residues can be used as raw materials. The catalyst resources are renewable and the manufacturing cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the gas chromatography-mass spectrometry (GC-MC) of the product after lignin depolymerization;
[0032] Figure 2 The full XPS spectrum of Nd2O3 / NSPHC provided by the present invention;
[0033] Figure 3 This is the XRD diagram of Nd2O3 / NSPHC provided by the present invention. DETAILED DESCRIPTION
[0034] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples described. The experimental methods for specific adjustments not specified in the following examples are selected according to the product specifications. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs.
[0035] Embodiment 1:
[0036] A novel catalyst for catalytic depolymerization of biomass and a preparation method thereof, comprising the following steps:
[0037] Step 1: Take some biomass, wash it, dry it at 80°C for 12 hours, cool it to room temperature and slice it, then put it into a video grinder for crushing, take it out and continue to grind it into biomass powder, put it in a vacuum bag for standby use; the biomass can be various agricultural wastes such as shells, stalks, stems, various forestry and grass wastes such as sawdust, branches, hay, and various crop processing residues such as sugarcane bagasse, rice husks, peanut shells, etc. In this embodiment, the biomass is sugarcane bagasse;
[0038] Step 2: Add appropriate amounts of biomass powder, calcium chloride, and a first catalyst to deionized water and stir to obtain a mixed precursor; the first catalyst is any one of thiourea, activated carbon, carbon nanotubes, urea, thioacetamide, and sodium sulfide. In this embodiment, the first catalyst is thiourea; the weight ratio of biomass powder: calcium chloride: first catalyst is 1:2:2;
[0039] Step 3: Rotate the mixed precursor to evaporate completely, transfer it to a container, and dry it at 85°C for 12 hours;
[0040] Step 4: The dried product is placed in a nickel crucible and placed in a tube furnace, filled with protective gas, with nitrogen as the protective gas, heated to 800° C. at a heating rate of 5° C. / min, and maintained for 2 hours to obtain a non-metallic catalyst crude product, i.e., a NSHPC crude product;
[0041] Step 5: After the crude non-metallic catalyst product is cooled, the crude non-metallic catalyst product is immersed in 1.0 mol / L dilute hydrochloric acid and stirred continuously for 6 hours, and then the mixed solution is filtered, and the filtered solid is washed with deionized water until the solid is neutral, and then dried in a vacuum at 60° C. to obtain a non-metallic catalyst, namely NSHPC;
[0042] Step 6: Calculate the required second catalyst based on the carbon loading ratio, take the corresponding mass of the second catalyst, add an appropriate amount of water to dissolve it, and obtain a second catalyst aqueous solution; in this embodiment, the second catalyst is Nd(NO3)3.
[0043] Step 7: Take an appropriate amount of the non-metallic catalyst (NSHPC) in step 5, add it to the second catalyst aqueous solution in step 6, then add appropriate amount of water, perform ultrasonic stirring to dissolve, and then immerse for 12 hours.
[0044] Step 8: Place the solution impregnated in step 7 in an oven and dry at 105°C for 12 hours;
[0045] Step nine: The dried solution in step eight is placed in a tube furnace for heat treatment, with nitrogen as the protective gas, heated to 450°C, with a heating rate of 5°C / min, and maintained at 450°C for 1 hour, finally obtaining a new catalyst, namely Nd2O3 / NSHPC.
[0046] Embodiment 2:
[0047] Compared with Example 1, the difference is that the second catalyst is Pr(NO)3, and Pr6O 11 / NSHPC.
[0048] Embodiment 3:
[0049] A method for using a novel catalyst for catalytic depolymerization of biomass
[0050] Add an appropriate amount of lignin and a catalyst for catalytic depolymerization of biomass into the solvent, and perform a degradation reaction at 180°C and an air pressure of 1.5 MPa, and the degradation and depolymerization is realized for 4 hours, wherein the solvent is any one of methanol, isopropanol, and ethanol; in this embodiment, the solvent is methanol, the volume of the solvent is 25 ml, the weight of lignin (the type of lignin is pp-one) is 100 mg, the weight of the catalyst is 20 mg, and the pressurized gas is oxygen.
[0051] Embodiment 4:
[0052] Compared with Example 3, the difference is that the temperature during the depolymerization reaction is 160°C.
[0053] Embodiment 5:
[0054] Compared with Example 3, the difference is that the temperature during the depolymerization reaction is 200°C.
[0055] Embodiment 6:
[0056] Compared with Example 3, the difference is that the depolymerization reaction time is 3 hours.
[0057] Embodiment 7:
[0058] Compared with Example 3, the difference is that the depolymerization reaction time is 5 hours.
[0059] Embodiment 8:
[0060] Determination of depolymerization products after catalytic depolymerization of lignin using biomass catalysts
[0061] After the degradation reaction is completed, the depolymerization products are analyzed quantitatively and directional by gas chromatography-mass spectrometry. Figure 1 The following is the gas chromatography-mass spectrometry diagram of the depolymerization product. Figure 1It can be seen that the depolymerization products are phenol, methyl benzoylformate, benzoic acid, and methyl benzoate.
[0062] Embodiment 9:
[0063] According to the usage scheme of Example 3, the new catalyst for catalytic depolymerization of biomass prepared in Example 1 and Example 2 was used to depolymerize lignin, respectively. At the same time, a blank group and a control group 1, a control group 2 and a control group 3 were set up, wherein the blank group did not add a catalyst to depolymerize lignin, the control group 1 added activated carbon for depolymerization, the control group 2 added NSHPC (NSHPC prepared in Example 1 of the present application) for depolymerization, and the control group 3 added Nd2O3 for depolymerization, and the depolymerization product yield and the overall conversion rate were calculated.
[0064] The quantitative analysis of the model molecular compound was performed by the LC-100 liquid chromatograph equipped by Wufeng Company. The liquid chromatograph was equipped with a UV xenon lamp detector, a 5μm C18 (250X4.6mm) chromatographic column, a column box temperature of 35°C, a mobile phase of acetonitrile: water = 6:4, and a flow rate of 1.0ml / min. The results are shown in Table 1.
[0065] The specific calculation formulas for product yield (%) and conversion rate (%) are as follows:
[0066] Conversion rate = (the amount of substrate substance remaining after the reaction / the amount of substrate substance before the reaction) x 100%.
[0067] Product yield = (molar amount of product / total molar amount of substrate) × 100%.
[0068] Table 1 Comparison of the performance of different catalysts for catalytic depolymerization of lignin
[0069]
[0070] As shown in Table 1, without adding any catalyst, the conversion rate of the substrate is only 5.05%. This shows that under these conditions, the stability of the substrate is relatively high.
[0071] Limitations of single activated carbon: When only activated carbon is used as a catalyst, the conversion effect of the lignin model molecule is not satisfactory, showing a low efficiency of 19.24%. Specifically, the conversion rate is low and the product yield is not ideal. Most of the model molecules fail to be converted into the expected aromatic monomers, but are converted into other byproducts or completely oxidized to CO2. The carbon balance results show that the nonspecificity of the conversion path is high.
[0072] Limitations of NSHPC carbon material catalysts: Although there was some improvement when using NSHPC carbon material as a catalyst, the conversion rate still remained at about 56%, and the product yield was also relatively limited, reflecting its limitations in catalytic selectivity.
[0073] Significant improvement in lanthanide metal loading: When lanthanide metals Pr or Nd were loaded on NSHPC carbon materials, the conversion efficiency experienced a qualitative leap, soaring to over 95%, reaching 95.14% and 97.82%, respectively. This change was accompanied by a significant increase in the yields of the target products phenol and acetophenone, reaching the range of 40%-60% and 20%-30%, respectively, which were significantly better than the performance before the metal was loaded. This directly indicates that the introduction of lanthanide metal oxides greatly enhanced the selectivity and efficiency of the catalyst in breaking the CO bond.
[0074] The superiority of Nd2O3 / NSHPC: further comparison with Pr6O 11 The performance of Nd2O3 / NSHPC and Nd2O3 / NSHPC was compared, and it was found that the latter showed better performance in both conversion rate and product yield. This difference is attributed to the higher apparent valence of the Nd element, which gives Nd2O3 a stronger electron attraction ability, which in turn may enhance the adsorption of the catalyst on the lignin model molecules and promote the effective contact and reaction between the model molecules and the catalyst surface, thereby achieving higher conversion efficiency and more precise selectivity, allowing more model molecules to be converted into target products rather than byproducts or CO2.
[0075] In summary, Nd2O3 / NSHPC, as an efficient catalyst, exhibits excellent conversion ability and product selectivity in the catalytic depolymerization of lignin model molecules, with a high conversion rate of more than 95% for lignin. It uses biomass resources such as sugarcane bagasse as a carrier to achieve resource recycling and has low manufacturing cost.
[0076] Embodiment 10:
[0077] XPS full spectrum analysis of Nd2O3 / NSHPC of Example 1
[0078] like Figure 2As shown in the figure, several significant features can be observed. First, through a detailed analysis of the O1s element spectrum, we confirmed that the successful loading of metal oxides not only enhanced the lattice oxygen characteristics of the material, but also significantly increased the content of oxygen elements, which directly proved that metal elements such as Nd have been effectively loaded on the NSHPC carrier. In addition, trace S element signals can still be detected in the spectrum, and these S elements mainly exist in the form of sulfonic acid sulfur, indicating that some sulfur components in the original material are retained during the loading process. It is worth noting that the relative content of N element increases after the metal oxide is loaded. This may be due to the secondary introduction of N2 as a protective gas during the calcination process, which promotes the combination of N element with metal oxide and effectively loads it on the surface of carbon material. On the other hand, high temperature conditions may also promote the formation of nitrides, which is confirmed by the newly appeared N element metal peak in the XPS spectrum, further emphasizing the key role of N element in the composite material. It helps to stabilize the structure of the material through close combination with the metal element, thereby significantly improving the catalytic activity of the catalyst.
[0079] Embodiment 11:
[0080] XRD spectrum analysis of Nd2O3- / NSHPC of Example 1
[0081] like Figure 3 As shown, several important diffraction peaks located near 21.5° and 43.4° can be observed, which correspond to the (002) plane diffraction of irregular porous carbon, the carbon peak generated by π-π stacking in the benzene ring structure, and the weak diffraction of the porous carbon (001) plane. It is worth noting that when Nd2O3 is loaded on NSHPC, the structural crystal form of the material changes significantly. Specifically, the metal peak of Nd2O3 shifts and overlaps with the diffraction peak of the carbon material. At the same time, the diffraction peak of carbon also shows a large shift, and the overall structure tends to be irregular or disordered. These phenomena together indicate that the Nd2O3 / NSHPC composite material may have a disordered amorphous structural feature, which may have a profound impact on its catalytic performance and provide a favorable structural basis for the efficient conversion of lignin model molecules.
[0082] Embodiment 12:
[0083] The novel catalyst for catalytic depolymerization of biomass prepared in Example 1 was used to depolymerize lignin according to the methods of Examples 3 to 5, and the overall conversion rate was calculated.
[0084] The quantitative analysis of the model molecular compound was performed by the LC-100 liquid chromatograph equipped by Wufeng Company. The liquid chromatograph was equipped with a UV xenon lamp detector, a 5μm C18 (250X4.6mm) chromatographic column, a column box temperature of 35°C, a mobile phase of acetonitrile: water = 6:4, and a flow rate of 1.0ml / min. The results are shown in Table 2.
[0085] The specific calculation formula of conversion rate (%) is as follows:
[0086] Conversion rate = (the amount of substrate substance remaining after the reaction / the amount of substrate substance before the reaction) x 100%.
[0087] Table 2 Comparison of the results of depolymerization of lignin by catalysts at different weight ratios
[0088] Serial number catalyst temperature Substrate Solvents time Conversion rate (%) Carbon Balance 1 blank 180 PP-one Methanol 4h 5.05 92.18 2 <![CDATA[Nd2O3 / NSHPC]]> 160 PP-one Methanol 4h 27.04 67.99 3 <![CDATA[Nd2O3 / NSHPC]]> 180 PP-one Methanol 4h 99.53 83.41 4 <![CDATA[Nd2O3 / NSHPC]]> 200 PP-one Methanol 4h 99.93 74.15
[0089] As shown in Table 2, the lignin model molecules were depolymerized at different temperatures using Nd2O3 / NSHPC catalyst, and the results are shown in Table 2. As shown in the table, when the temperature was 160 degrees, the conversion rate of the lignin model molecule was 27%. The carbon balance was 67.99%. When the temperature was 180 degrees, the substrate conversion rate reached 99.53%, and the carbon balance was 83.4%. When the temperature was 200 degrees, the substrate conversion rate was 99.83%, and the carbon balance was 74.51%. It can be found that with the increase in temperature, the substrate conversion rate gradually increased. However, when the temperature rose from 180 degrees to 200 degrees, the substrate conversion rate did not increase significantly. It can be seen that the optimal reaction temperature is 180 degrees.
[0090] Embodiment 13:
[0091] The novel catalyst for catalytic depolymerization of biomass prepared in Example 1 was used to depolymerize lignin according to the methods of Example 3, Example 6 and Example 7, and the overall conversion rate was calculated.
[0092] The quantitative analysis of the model molecular compound was performed by the LC-100 liquid chromatograph equipped by Wufeng Company. The liquid chromatograph was equipped with a UV xenon lamp detector, a 5μm C18 (250X4.6mm) chromatographic column, a column box temperature of 35°C, a mobile phase of acetonitrile: water = 6:4, and a flow rate of 1.0ml / min. The results are shown in Table 2.
[0093] The specific calculation formula of conversion rate (%) is as follows:
[0094] Conversion rate = (the amount of substrate substance remaining after the reaction / the amount of substrate substance before the reaction) x 100%.
[0095] Table 3 Comparison of depolymerization of lignin by new catalysts at different times
[0096] Serial number catalyst temperature Substrate Solvents time Conversion rate (%) Carbon Balance 1 blank 180 PP-one Methanol 4 hours 5.05 92.18 2 <![CDATA[Nd2O3 / NSHPC]]> 180 PP-one Methanol 3 hours 96.25 68.98 3 <![CDATA[Nd2O3 / NSHPC]]> 180 PP-one Methanol 4 hours 99.53 83.41 4 <![CDATA[Nd2O3 / NSHPC]]> 180 PP-one Methanol 5 hours 95.68 76.25
[0097] The Nd2O3 / NSHPC catalyst was used to depolymerize the lignin model molecule at different temperatures, and the results are shown in Table 3. It can be seen from the table that when the reaction time is 3 hours, the bottom conversion rate is 96.25% and the carbon balance is 68.98%. When the reaction time is 4h, the substrate conversion rate is 99.53% and the carbon balance is 83.41%. When the reaction time is 5 hours, the substrate conversion rate is 95.68% and the carbon balance is 76.25%. The results show that with the extension of the reaction time, the substrate conversion first increases and then decreases. It can be seen that the optimal reaction time is 4 hours.
[0098] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the present invention.
Claims
1. A method for preparing a novel catalyst for catalytic depolymerization of biomass, characterized in that: The following steps are involved: Step 1: Take some biomass, wash it, dry it, cool it to room temperature, and then grind it into biomass powder for later use; Step 2: adding an appropriate amount of biomass powder, calcium chloride, and a first catalyst to deionized water, and stirring to obtain a mixed precursor; Step 3: Rotate the mixed precursor to evaporate, transfer to a container after the water is completely evaporated, and dry; Step 4: Put the dried product into a nickel crucible and place it in a tube furnace, fill it with protective gas, and heat it to obtain a crude non-metallic catalyst product; Step 5: After the crude non-metallic catalyst product is cooled, the crude non-metallic catalyst product is immersed in dilute hydrochloric acid and continuously stirred, and then the mixed solution is filtered, and the filtered solid is washed with deionized water until the solid is neutral, and then placed in a vacuum dry to obtain a non-metallic catalyst; Step 6: Take a corresponding mass of the second catalyst, add an appropriate amount of water to dissolve it, and obtain a second catalyst aqueous solution; Step 7: Take an appropriate amount of the non-metallic catalyst in step 5, add it to the second catalyst aqueous solution in step 6, then add appropriate amount of water, perform ultrasonic stirring to dissolve and then immerse; Step 8: Drying the solution impregnated in step 7; Step nine: heat-treating the dried solution in step eight, and simultaneously injecting a protective gas for calcination, to finally obtain a new catalyst.
2. The method for preparing the novel catalyst for catalytic depolymerization of biomass according to claim 1, characterized in that: The first catalyst is thiourea.
3. The method for preparing the novel catalyst for catalytic depolymerization of biomass according to claim 1, characterized in that: The weight ratio of biomass powder:calcium chloride:first catalyst is 1:2:
2.
4. The method for preparing the novel catalyst for catalytic depolymerization of biomass according to claim 1, characterized in that: The second catalyst is Nd(NO3)3 or Pr6O 11 .
5. A novel catalyst for catalytic depolymerization of biomass, prepared by the preparation method of a novel catalyst for catalytic depolymerization of biomass according to any one of claims 1 to 4.
6. The method for using the novel catalyst for catalytic depolymerization of biomass according to claim 5, characterized in that: Lignin and the novel catalyst according to claim 5 are added into a solvent to carry out a depolymerization reaction.
7. The method for using the novel catalyst for catalytic depolymerization of biomass according to claim 6, characterized in that: The temperature during the depolymerization reaction is 160°C-200°C.
8. The method for using the novel catalyst for catalytic depolymerization of biomass according to claim 7, characterized in that: The gas pressure during the depolymerization reaction was 1.5 MPa.
9. The method for using the novel catalyst for catalytic depolymerization of biomass according to claim 6, characterized in that: The depolymerization reaction time is 3 hours to 5 hours.