Nanometer titanium dioxide composite hydroxyapatite photocatalytic material, preparation method thereof and photo-decomposition cigarette tar filter part
The nano-titanium dioxide composite hydroxyapatite photocatalytic material addresses the issue of secondary pollution and reduced efficiency in cigarette smoke filters by effectively decomposing tar and nicotine into harmless compounds, enhancing air purification.
Patent Information
- Application Number
- CN202411169971.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
AI Technical Summary
Existing cigarette smoke filters fail to effectively decompose tar and nicotine, leading to secondary pollution and reduced purification efficiency due to desorption and microbial growth, which affects user experience.
A photocatalytic material of nano-titanium dioxide composite hydroxyapatite is prepared by a specific method, incorporating hydroxyapatite to increase surface area and distribute TiO2 uniformly, allowing electron-hole pair generation under UV light to decompose tar and nicotine into volatile compounds.
The photocatalytic material efficiently decomposes tar and nicotine into odorless substances, improving air purification by reducing secondary pollution and enhancing the filtration effect.
Smart Images

Figure CN119056473A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photocatalysis, in particular to a photocatalytic material of nano-titanium dioxide composite hydroxyapatite and a preparation method thereof and a photodecomposition cigarette tar filter. Background Art
[0002] The composition of cigarette smoke is complex, and the main components include PM2.5, tar, nicotine, etc. The filter materials for cigarette smoke provided by related technologies can usually only intercept and adsorb pollutants. As the pollutants are gradually deposited on the adsorption materials, the typical smoke smell contained in the tar in the cigarette smoke will be desorbed into the air again, causing secondary pollution. At the same time, the tar deposited on the adsorption material also provides nutrition for the reproduction of microorganisms. After long-term use, the metabolism of microorganisms on the adsorption material produces sour taste, which reduces the purification effect and poor user experience.
[0003] In view of this, the present disclosure provides a photocatalytic material that can effectively decompose tobacco tar and nicotine to improve the secondary pollution problem of desorption and enhance the purification effect. Summary of the invention
[0004] The purpose of the present invention is to provide a photocatalytic material of nano-titanium dioxide composite hydroxyapatite and a preparation method thereof and a photodecomposition tar filter. The photocatalytic material of nano-titanium dioxide composite hydroxyapatite prepared by the preparation method can effectively decompose tar and nicotine under the action of photocatalysis, decomposing them into volatile, odorless substances, thereby improving the secondary pollution problem caused by the desorption of tar and improving the air purification effect. The photodecomposition tar filter with the photocatalytic material of nano-titanium dioxide composite hydroxyapatite can fully decompose tar, improve the secondary pollution problem caused by the desorption of tar and improve the air purification effect.
[0005] The present invention is achieved in that:
[0006] In a first aspect, the present invention provides a method for preparing a photocatalytic material of nano-titanium dioxide composite hydroxyapatite, comprising:
[0007] At a first preset temperature and under stirring conditions, adding a diammonium phosphate solution dropwise to a mixed solution of calcium chloride and titanium chloride to obtain a first precipitate;
[0008] The first precipitate is allowed to stand for aging at a second preset temperature, and then filtered to obtain a first filtrate;
[0009] The first filtered product is washed to neutrality, and then dried and ground;
[0010] The ground first filtrate is subjected to a hydrothermal reaction at a third preset temperature, filtered, and washed to obtain titanium dioxide composite hydroxyapatite;
[0011] The suspension of titanium dioxide composite hydroxyapatite and the emulsion are mixed to prepare a suspension;
[0012] The suspension is allowed to adhere to the surface of the porous material particles and dry and solidify.
[0013] In an optional embodiment, the Ti / (Ca+Ti) in the mixed solution of calcium chloride and titanium chloride is 0.05 to 3.0; and / or,
[0014] The molar ratio of P in the ammonium dihydrogen phosphate solution to Ca in the mixed solution of calcium chloride and titanium chloride is 0.5 to 0.7.
[0015] In an optional embodiment, the diammonium phosphate solution is added dropwise to the mixed solution of calcium chloride and titanium chloride at a dripping rate of 1.0 to 50 g / min.
[0016] In an optional embodiment, the pH of the ammonium dihydrogen phosphate solution and the mixed solution of calcium chloride and titanium chloride is 8.5-9.5; and / or,
[0017] The first preset temperature is 35-80° C.; and / or,
[0018] The second preset temperature is 35-80° C.; and / or,
[0019] The aging time is 1 to 24 hours; and / or,
[0020] The temperature of the first filtrate which is dried and washed to be neutral is 60-150° C.; and / or,
[0021] The mesh size of the first filtrate after grinding is 40 to 400 meshes.
[0022] In an optional embodiment, the ground first filtrate is mixed with water for hydrothermal reaction, and the mass ratio of the ground first filtrate to water is (0.01-0.5):1; and / or,
[0023] The pH of the ground first filtrate during hydrothermal reaction is 8.5 to 9.5; and / or,
[0024] The third preset temperature is 180-250° C.; and / or,
[0025] The reaction time of the hydrothermal reaction is 4 to 24 hours; and / or,
[0026] After hydrothermal reaction, filtration and washing, the mixture is dried at a temperature of 60 to 150° C. for 4 to 24 hours to obtain titanium dioxide composite hydroxyapatite.
[0027] In an optional embodiment, the emulsion includes styrene acrylic emulsion and acrylic emulsion, wherein the mass ratio of styrene acrylic emulsion to acrylic emulsion is (1-10):1, and the glass transition temperature of the emulsion is -5-10°C; and / or,
[0028] The mass ratio of the emulsion to the suspension of titanium dioxide-composite hydroxyapatite is (0.03-0.2):1; and / or,
[0029] The preparation method of the suspension of titanium dioxide composite hydroxyapatite comprises: mixing the titanium dioxide composite hydroxyapatite and water in a mass ratio of (0.3-0.9):1 by ball milling.
[0030] In an optional embodiment, the styrene acrylic emulsion has a solid content of 40-50%, a pH of 6-11, a viscosity of 20-3000 mPa.S, a surface tension of 30-70 mN / m, a particle size of 80-200 nm, and a glass transition temperature of -100-50°C.
[0031] In an optional embodiment, the acrylic emulsion has a solid content of 45-50%, a pH of 6-9, a viscosity of 10-1000 mPa.S, a surface tension of 30-70 mN / m, a particle size of 100-400 nm, and a glass transition temperature of -40-20°C.
[0032] In an optional embodiment, the mass ratio of the suspension to the porous material particles is (0.2-1.2):1; and / or,
[0033] The porous material particles include: at least one of alumina particles, activated carbon particles, molecular sieve particles and silica gel particles; and / or,
[0034] The particle size of porous material particles is 1.0-5.0mm, and the specific surface area is ≥150m / g 2 , water absorption ≥ 21%, crushing strength ≥ 150N, bulk density 0.4~0.9g / cm 3 and / or,
[0035] After the suspension is attached to the surface of the porous material particles, the drying temperature is 60-150° C.; and / or,
[0036] The method for attaching the suspension to the porous material particles comprises: stirring the porous material particles at a rotation speed of 15-25 r / min, and then atomizing and spraying the suspension onto the surface of the porous material particles.
[0037] In a second aspect, the present invention provides a nano-titanium dioxide composite hydroxyapatite photocatalytic material, which is prepared by the preparation method of the nano-titanium dioxide composite hydroxyapatite photocatalytic material of any one of the aforementioned embodiments.
[0038] In a third aspect, the present invention further provides a photodecomposition smoke tar filter, which comprises: a stacked HEPA layer, an activated carbon layer and an LED substrate layer, the aforementioned nano-titanium dioxide composite hydroxyapatite photocatalytic material being attached to the HEPA layer and / or the activated carbon layer.
[0039] In an optional embodiment, the HEPA layer includes a PET layer stacked in sequence with a photocatalytic material loaded with nano-titanium dioxide composite hydroxyapatite, a middle layer formed by melt-blowing a PP masterbatch of a photocatalytic material attached with nano-titanium dioxide composite hydroxyapatite, a hindered amine PP masterbatch, and a hindered amine-modified PP non-woven fabric layer; wherein the side of the PET layer facing away from the middle layer is the air inlet side.
[0040] In an optional embodiment, the activated carbon layer includes a hindered amine-modified PP plastic grid layer and a columnar activated carbon layer modified with a photocatalytic material of nano-titanium dioxide composite hydroxyapatite, which are stacked in sequence.
[0041] In an optional embodiment, the LED substrate layer includes a high thermal conductivity aluminum nitride substrate and UVC-LED lamp beads. The high thermal conductivity aluminum nitride substrate has multiple assembly areas, which are respectively distributed in different areas of the high thermal conductivity aluminum nitride substrate, and the assembly areas are provided with assembly holes, and the UVC-LED lamp beads are assembled in the assembly holes.
[0042] The present invention includes the following beneficial effects:
[0043] The preparation method of the photocatalytic material of nano-titanium dioxide composite hydroxyapatite of the present invention increases the specific surface area of the photocatalytic material by introducing a hydroxyapatite carrier, so that the tar and nicotine molecules are quickly adsorbed in the photocatalytic material, and at the same time, the titanium dioxide uniformly distributed in the pores of the hydroxyapatite is used to expose more active sites, and under the light energy excitation of UVC ultraviolet light, the TiO2 in the hydroxyapatite generates electron hole pairs (e- / h+), which react with water molecules to generate hydroxyl radicals (·OH) with strong oxidizing properties to attack the tar and nicotine molecules, decomposing them into smaller, more volatile, odor-free compounds, such as carbon dioxide, water and other oxygen-containing compounds, thereby improving the secondary pollution problem caused by the desorption of tar and improving the air purification effect. Hydroxyapatite itself has a high adsorption capacity, and can bind the odor molecules of cigarettes on the catalyst surface, increase their residence time on the catalyst surface, and thus improve the photocatalytic degradation efficiency.
[0044] The nano-titanium dioxide composite hydroxyapatite photocatalytic material of the present invention is prepared by the above-mentioned preparation method. The photocatalytic material can effectively decompose tobacco tar, improve the secondary pollution problem caused by tobacco tar desorption, and improve the air purification effect.
[0045] The photodecomposition of tobacco tar filter of the present invention has a photocatalytic material of nano-titanium dioxide composite hydroxyapatite attached to at least one of the HEPA layer and the activated carbon layer. On the one hand, tobacco tar can be adsorbed and captured by the HEPA layer and the activated carbon layer. On the other hand, the photocatalytic material of nano-titanium dioxide composite hydroxyapatite can be used to effectively decompose tobacco tar, thereby improving the secondary pollution problem caused by desorption of tobacco tar and improving the air purification effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0047] Figure 1 is a cross-sectional view of the photodegradable tobacco tar filter of the present invention;
[0048] Figure 2 is the Fourier infrared spectrum of Experimental Example 2 of the present invention;
[0049] Figure 3 This is a trend diagram of the color change of cigarette tar in Experimental Example 4 of the present invention.
[0050] Reference numerals:
[0051] 010-photodecomposition smoke tar filter; 100-HEPA layer; 200-activated carbon layer; 300-LED substrate layer; 310-high thermal conductivity aluminum nitride substrate; 320-UVC-LED lamp beads. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0053] The present invention provides a method for preparing a photocatalytic material of nano-titanium dioxide composite hydroxyapatite, comprising:
[0054] At a first preset temperature and under stirring conditions, adding a diammonium phosphate solution dropwise to a mixed solution of calcium chloride and titanium chloride to obtain a first precipitate;
[0055] The first precipitate is allowed to stand for aging at a second preset temperature, and then filtered to obtain a first filtrate;
[0056] The first filtered product is washed to neutrality, and then dried and ground;
[0057] The ground first filtrate is subjected to a hydrothermal reaction at a third preset temperature, filtered, and washed to obtain titanium dioxide composite hydroxyapatite;
[0058] The suspension of titanium dioxide composite hydroxyapatite and the emulsion are mixed to prepare a suspension;
[0059] The suspension is allowed to adhere to the surface of the porous material particles and dry and solidify.
[0060] The preparation method introduces hydroxyapatite carrier to increase the specific surface area of the photocatalytic material, so that the tar and nicotine molecules are quickly adsorbed in the photocatalytic material. At the same time, the titanium dioxide evenly distributed in the pores of hydroxyapatite is used to expose more active sites. Under the light energy excitation of UVC ultraviolet light, the TiO2 in the hydroxyapatite generates electron-hole pairs (e- / h+), which react with water molecules to generate hydroxyl radicals (·OH) with strong oxidizing properties to attack the tar and nicotine molecules, decomposing them into smaller, more volatile, odor-free compounds, such as carbon dioxide, water and other oxygen-containing compounds, thereby improving the secondary pollution problem caused by the desorption of tar and improving the air purification effect. Hydroxyapatite itself has a high adsorption capacity, which can bind the odor molecules of cigarettes to the catalyst surface, increase their residence time on the catalyst surface, and thus improve the efficiency of photocatalytic degradation.
[0061] Optionally, the Ti / (Ca+Ti) in the mixed solution of calcium chloride and titanium chloride is 0.05 to 3.0, for example: 0.05, 0.1, 0.3, 0.5, 0.9, 1.0, 1.2, 1.5, 1.8, 2, 2.3, 2.5, 2.7, 3, etc., which are not specifically limited here. By optimizing the relative content of Ti, it is beneficial to reduce the particle size of the formed titanium dioxide. On the one hand, it ensures that small particles of nano titanium dioxide can be more evenly dispersed on the surface of hydroxyapatite, that is, good dispersibility is obtained to expose more active sites and improve the effect of catalytic decomposition; on the other hand, it can further ensure a sufficiently large specific surface area so that the prepared photocatalyst has a stronger and more effective adsorption effect. In this way, when the photocatalyst prepared by the preparation method is used to catalytically remove tobacco tar and nicotine, it can efficiently decompose while efficiently adsorbing, effectively improving the efficiency and effect of purification.
[0062] Optionally, the molar ratio of P in the ammonium dihydrogen phosphate solution to Ca in the mixed solution of calcium chloride and titanium chloride is 0.5 to 0.7, for example: 0.5, 0.55, 0.6, 0.65, 0.7, etc., which is not specifically limited here. By optimizing the molar ratio between P and Ca, it is beneficial to obtain hydroxyapatite with a larger specific surface area, which on the one hand improves the adsorption effect of polluted gases, and on the other hand ensures that more nano-sized titanium dioxide is attached to the hydroxyapatite to improve the decomposition effect of polluted gases.
[0063] Optionally, the dripping rate of the ammonium dihydrogen phosphate solution to the mixed solution of calcium chloride and titanium chloride is 1.0 to 50 g / min, for example: 1 g / min, 2 g / min, 5 g / min, 8 g / min, 10 g / min, 12 g / min, 15 g / min, 18 g / min, 20 g / min, 23 g / min, 25 g / min, 28 g / min, 30 g / min, 33 g / min, 35 g / min, 38 g / min, 40 g / min, 42 g / min, 45 g / min, 48 g / min,
[0064] Optimizing the dripping rate of ammonium dihydrogen phosphate is conducive to improving the problem of solidification, thereby ensuring the subsequent preparation of hydroxyapatite with a large specific surface area, and ensuring that hydroxyapatite can evenly attach a large amount of nano-sized titanium dioxide, ensuring the adsorption, catalytic efficiency and effect of the prepared photocatalyst.
[0065] Optionally, the pH of the ammonium dihydrogen phosphate solution and the mixed solution of calcium chloride and titanium chloride is 8.5-9.5, for example: 8.5, 8.8, 9.0, 9.3, 9.5, etc., which are not specifically limited here. Optimizing the pH of the ammonium dihydrogen phosphate solution and the mixed solution of calcium chloride and titanium chloride can improve the problem of agglomeration, thereby ensuring the subsequent preparation of hydroxyapatite with a large specific surface area, and ensuring that the hydroxyapatite can evenly attach a large amount of nano-sized titanium dioxide, ensuring the adsorption, catalytic efficiency and effect of the prepared photocatalyst.
[0066] Optionally, the first preset temperature is 35-80°C, for example, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc., which is not specifically limited here.
[0067] It should be noted that when the ammonium dihydrogen phosphate solution is added dropwise to the mixed solution of calcium chloride and titanium chloride, it can be carried out under the condition of heating in a water bath, so as to stably and reliably control the reaction temperature.
[0068] Optionally, the second preset temperature is 35-80°C, for example, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc., which is not specifically limited here.
[0069] Optimizing the temperature and static aging of the mixture of ammonium dihydrogen phosphate solution and the mixed solution of calcium chloride and titanium chloride is beneficial to improving the agglomeration problem, thereby ensuring the subsequent preparation of hydroxyapatite with a large specific surface area, and ensuring that the hydroxyapatite can evenly attach a large amount of nano-sized titanium dioxide, thereby ensuring the adsorption, catalytic efficiency and effect of the prepared photocatalyst.
[0070] Optionally, the standing aging time is 1 to 24 hours, for example: 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, etc., without specific limitation here.
[0071] Optionally, the temperature of the dried, cleaned, neutral first filtrate is 60-150°C, for example, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc., which is not specifically limited here.
[0072] Optionally, the mesh number of the first filtrate after grinding is 40 to 400 meshes, for example: 40 meshes, 80 meshes, 120 meshes, 150 meshes, 180 meshes, 200 meshes, 250 meshes, 300 meshes, 350 meshes, 400 meshes, etc., which are not specifically limited here. Controlling the particles of the first filtrate after grinding to be larger is conducive to ensuring the specific surface area of the first filtrate, and is conducive to ensuring that a sufficient amount of nano-scale titanium dioxide can be attached to hydroxyapatite, while ensuring the adsorption of the photocatalyst, and improving the catalytic decomposition effect of the photocatalyst.
[0073] Optionally, the ground first filtrate and water are mixed for a hydrothermal reaction, and the mass ratio of the ground first filtrate and water is (0.01-0.5):1, for example: 0.01:1, 0.02:1, 0.05:1, 0.08:1, 0.1:1, 0.15:1, 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, etc., which is not specifically limited here.
[0074] It should be noted that the water mixed with the first filtrate may be deionized water.
[0075] Optionally, the pH of the ground first filtrate during the hydrothermal reaction is 8.5 to 9.5, for example, 8.5, 8.8, 9.0, 9.3, 9.5, etc., which is not specifically limited here.
[0076] Optionally, the third preset temperature is 180-250°C, for example, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, etc., which is not specifically limited here.
[0077] Optimizing the pH and reaction temperature of the hydrothermal reaction can ensure that the hydrothermal reaction is more thorough and improve the efficiency of the reaction. It can also ensure that the prepared titanium dioxide composite hydroxyapatite has a larger specific surface area and ensure a sufficient amount of titanium dioxide, thereby improving the adsorption, catalytic efficiency and effect of the photocatalyst.
[0078] Optionally, the reaction time of the hydrothermal reaction is 4 to 24 h, for example: 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, 21 h, 22 h, 23 h, 24 h, etc., without specific limitation herein.
[0079] Optionally, after hydrothermal reaction, filtration and washing, the titanium dioxide composite hydroxyapatite is obtained by drying for 4 to 24 hours (for example, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, etc., not specifically limited here) at a temperature of 60 to 150°C (for example, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc., not specifically limited here). The appropriate drying temperature can ensure that titanium dioxide is stably attached to hydroxyapatite, thereby ensuring good catalytic and decomposition effects.
[0080] Optionally, the emulsion includes styrene acrylic emulsion and acrylic emulsion, wherein the mass ratio of styrene acrylic emulsion to acrylic emulsion is (1-10):1, for example: 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc., which are not specifically limited herein; the glass transition temperature of the emulsion is -5-10°C, for example: -5°C, -4°C, -3°C, -2°C, -1°C, 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, etc., which are not specifically limited herein.
[0081] Optionally, the mass ratio of the emulsion and the suspension of titanium dioxide composite hydroxyapatite is (0.03-0.2):1, for example: 0.03:1, 0.05:1, 0.08:1, 0.1:1, 0.12:1, 0.15:1, 0.17:1, 0.2:1, etc., which is not specifically limited here.
[0082] Optionally, the preparation method of the suspension of titanium dioxide composite hydroxyapatite includes: mixing titanium dioxide composite hydroxyapatite and water by ball milling in a mass ratio of (0.3-0.9):1, for example: 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, etc.
[0083] It should be noted that the water mixed with the titanium dioxide composite hydroxyapatite may be deionized water.
[0084] Optionally, the ball milling time is 4 to 24 h, for example: 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, etc., which is not specifically limited here.
[0085] Optionally, the solid content of the styrene-acrylic emulsion is 40-50% (for example: 40%, 42%, 45%, 48%, 50%, etc., not specifically limited herein), the pH is 6-11 (for example: 6, 7, 8, 9, 10, 11, etc., not specifically limited herein), and the viscosity is 20-3000 mPa.S (for example: 20 mPa.S, 50 mPa.S, 100 mPa.S, 200 mPa.S, 500 mPa.S, 1000 mPa.S, 1200 mPa.S, 1500 mPa.S, 1700 mPa.S, 2000 mPa.S, 2300 mPa.S, 2500 mPa.S,
[0086] 2700mPa.S, 3000mPa.S, etc., are not specifically limited herein), the surface tension is 30-70mN / m (for example: 30mN / m, 40mN / m, 50mN / m, 60mN / m, 70mN / m, etc., are not specifically limited herein), the particle size is 80-200nm (for example: 80nm, 90nm, 100nm, 120nm, 150nm, 180nm, 200nm, etc., are not specifically limited herein), and the glass transition temperature is -100-50℃ (for example: -100℃, -90℃, -80℃, -70℃, -60℃, -50℃, -40℃, -30℃, -20℃, -10℃, 0℃, 10℃, 20℃, 30℃, 40℃, 50℃, etc., are not specifically limited herein).
[0087] Styrene acrylic emulsion includes styrene acrylic copolymer emulsion, or other glues whose property parameters meet the above range, such as PU (Polyurethane), PVA (Polyvinyl Alcohol), VAE (Vinyl Acetate Ethylene Copolymer), etc.
[0088] Optionally, the acrylic emulsion includes an acrylic ester emulsion having a solid content of 45 to 50% (e.g., 45%, 46%, 47%, 48%, 49%, 50%, etc., not specifically limited herein), a pH of 6 to 9 (e.g., 6, 7, 8, 9, etc., not specifically limited herein), and a viscosity of 10 to 1000 mPa.S (e.g., 10 mPa.S, 20 mPa.S, 50 mPa.S, 70 mPa.S, 100 mPa.S, 200 mPa.S, 300 mPa.S, 400 mPa.S, 500 mPa.S, 600 mPa.S, 700 mPa.S, 800 mPa.S, 900 mPa.S, 1000 mPa.S, etc., not specifically limited herein). The surface tension is 30-70 mN / m (for example, 30 mN / m, 40 mN / m, 50 mN / m, 60 mN / m, 70 mN / m, etc., which are not specifically limited herein), the particle size is 100-400 nm (for example, 100 nm, 120 nm, 150 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm, 330 nm, 350 nm, 370 nm, 400 nm, etc., which are not specifically limited herein), and the glass transition temperature is -40-20°C (for example, -40°C, -30°C, -20°C, -10°C, 0°C, 10°C, 20°C, etc., which are not specifically limited herein).
[0089] Optionally, the mass ratio of the suspension to the porous material particles is (0.2-2):1, for example: 0.2:1, 0.3:1, 0.5:1, 0.7:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.5:1, 1.8:1, 2:1; preferably, (0.2-1.2):1, which is not specifically limited here.
[0090] Optionally, the porous material particles include at least one of aluminum oxide particles, activated carbon particles, molecular sieve particles and silica gel particles.
[0091] Optionally, the porous material particles have a particle size of 1.0-5.0 mm (for example, 1.0 mm, 2.0 mm, 3.0 mm, 4.0 mm, 5.0 mm, etc., not specifically limited here), and a specific surface area of ≥150 m / g 2 (For example: 150m / g 2 、155m / g 2 、160m / g 2etc., not specifically limited here), water absorption ≥21% (e.g. 21%, 22%, 23%, 24%, etc., not specifically limited here), crushing strength ≥150N (e.g. 150N, 155N, 160N, etc., not specifically limited here), bulk density 0.4-0.9g / cm 3 (For example: 0.4g / cm 3 , 0.5g / cm 3 , 0.6g / cm 3 , 0.7g / cm 3 , 0.8g / cm 3 , 0.9g / cm 3 etc., not specifically limited here).
[0092] Optionally, after the suspension is attached to the surface of the porous material particles, the drying temperature is 60-150°C, for example: 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, etc., which are not specifically limited here. The appropriate drying temperature can ensure that the titanium dioxide composite hydroxyapatite is stably and reliably attached to the porous material particles, thereby ensuring good catalytic and decomposition effects.
[0093] Optionally, the method of attaching the suspension to the porous material particles includes: stirring the porous material particles at a rotation speed of 15-25r / min (for example: 15r / min, 17r / min, 20r / min, 22r / min, 25r / min, etc., not specifically limited here), and then atomizing the suspension and spraying it onto the surface of the porous material particles.
[0094] For example, the suspension can be attached to the porous material particles by spraying, coating, etc. through equipment such as a coating machine, a sprayer, and a coating machine, which is not specifically limited here.
[0095] Please refer to Figure 1 The present disclosure also provides a photodecomposition smoke tar filter 010, which includes: a stacked HEPA layer 100, an activated carbon layer 200 and an LED substrate layer 300, and the above-mentioned nano-titanium dioxide composite hydroxyapatite photocatalytic material is attached to the HEPA layer and / or the activated carbon layer. The nano-titanium dioxide composite hydroxyapatite photocatalytic material is attached to at least one of the HEPA layer and the activated carbon layer. On the one hand, the smoke tar can be adsorbed and captured by the HEPA layer and the activated carbon layer, and on the other hand, the nano-titanium dioxide composite hydroxyapatite photocatalytic material can be used to effectively decompose the smoke tar, improve the secondary pollution problem caused by the desorption of the smoke tar, and improve the air purification effect.
[0096] Optionally, the photocatalytic material of nano-titanium dioxide composite hydroxyapatite can be loaded on the HEPA layer and the activated carbon layer by melt-blowing.
[0097] Optionally, the preparation method of the HEPA layer of the photocatalytic material attached with nano-titanium dioxide composite hydroxyapatite includes: folding the three layers of material after hot pressing or spraying composite with hot melt adhesive powder, that is, the HEPA layer can be a wavy plate structure; one of the outer layers is a PET layer of the photocatalytic material loaded with nano-titanium dioxide composite hydroxyapatite, the middle layer is formed by melt-blowing the PP masterbatch of the photocatalytic material attached with nano-titanium dioxide composite hydroxyapatite and the hindered amine PP masterbatch, and the PP masterbatch is blended, and the other outer layer is a hindered amine modified PP non-woven fabric.
[0098] Optionally, a HEPA layer of photocatalytic material attached with nano-titanium dioxide composite hydroxyapatite can be arranged on the air inlet side of the photodecomposition of tobacco tar filter. The airflow first enters through the PET surface, then to the melt-blown surface, and is blown out from the PP surface, thereby effectively intercepting particulate matter and tobacco tar. After being intercepted, the tobacco tar adheres to and penetrates into the PET and melt-blown fiber layers respectively, and is quickly decomposed into harmless substances by the photocatalytic material of nano-titanium dioxide composite hydroxyapatite. At the same time, hindered amines are added to the melt-blown material itself, which can simultaneously play the role of antibacterial and anti-UV, preventing the growth of microorganisms and material aging.
[0099] Optionally, the preparation method of the activated carbon layer attached with the photocatalytic material of nano-titanium dioxide composite hydroxyapatite includes: bonding two materials by pressure-sensitive adhesive; one layer is a PP plastic mesh layer modified by a hindered amine and the other layer is a columnar activated carbon layer modified by the photocatalytic material of nano-titanium dioxide composite hydroxyapatite (i.e., the surface and gap of the columnar activated carbon are attached with the photocatalytic material of nano-titanium dioxide composite hydroxyapatite), wherein the modified activated carbon is uniformly bonded to the surface of the PP plastic mesh. The activated carbon layer attached with the photocatalytic material of nano-titanium dioxide composite hydroxyapatite can rely on the activated carbon to quickly absorb small molecular gaseous pollutants generated during the combustion of cigarettes, such as benzene, aldehydes, esters, acids, etc., and then the photocatalytic material of nano-titanium dioxide composite hydroxyapatite attached with the activated carbon is quickly decomposed into harmless substances, and the hindered amine-modified PP plastic mesh can prevent material aging caused by ultraviolet light irradiation.
[0100] Optionally, the LED substrate layer 300 includes a high thermal conductivity aluminum nitride substrate 310 and UVC-LED lamp beads 320. The high thermal conductivity aluminum nitride substrate is evenly and neatly punched with assembly holes (the diameter of the assembly holes can be selected as needed, for example: 2mm, 3mm, etc.), and the spacing distance between the assembly holes can be set as needed, for example: 1mm, 1.2mm, etc., and the UVC-LED lamp beads are assembled at the assembly holes.
[0101] In some embodiments, each 4500 mm of the high thermal conductivity aluminum nitride substrate 2 The area needs to be reserved for 5 areas of 25mm2 The assembly area is used to embed UVC-LED lamp beads with length, width and height dimensions of 3.5mm×3.5mm×1.0mm, and the positions of the above five areas are respectively at the upper left, upper right, center, lower left and lower right. The assembly holes in other areas of the high thermal conductivity aluminum nitride substrate are not equipped with lamp beads for ventilation, that is, it can effectively ensure that the airflow passes through the LED substrate layer smoothly and reduce the wind resistance of the accessories. Of course, in other embodiments, the number of assembly areas can be increased or decreased as needed; the size of the high thermal conductivity aluminum nitride substrate and the size of the assembly area can be increased or decreased as needed.
[0102] Optionally, the UVC-LED lamp beads can be assembled by gold-tin eutectic welding to improve the bonding strength and thermal conductivity of the lamp beads and the substrate. When using the photodecomposition of smoke tar filter, ultraviolet light can fully radiate the HEPA layer and the activated carbon layer through the PP plastic mesh holes, so that the photocatalyst (i.e., the photocatalytic material of nano-titanium dioxide composite hydroxyapatite) can fully exert its catalytic decomposition effect.
[0103] Optionally, the gaps between adjacent sides of the HEPA layer, the activated carbon layer and the LED substrate layer may be 1.0 to 5.0 mm, for example, 1.0 mm, 2.0 mm, 3.0 mm, 4.0 mm, 5.0 mm, etc., which are not specifically limited here.
[0104] Optionally, the three-layer structure consisting of the HEPA layer, the activated carbon layer and the LED substrate layer can be fixed by wrapping with paper or aluminum frames.
[0105] The present invention is further described in detail below in conjunction with embodiments.
[0106] Example 1
[0107] Step 1: According to the P / Ca molar ratio of 0.6, weigh calcium chloride and ammonium dihydrogen phosphate in a 1000mL beaker, add 250mL of deionized water to the beaker, prepare calcium chloride and ammonium dihydrogen phosphate solutions (solution B), stir until completely dissolved and set aside. Then, according to the molar ratio of Ti / (Ca+Ti) equal to 0.1, add titanium chloride solution to the calcium chloride solution under ice bath conditions, stir evenly and set aside (mixed solution A). Finally, adjust the mixed solution A and solution B to pH = 9.0 with ammonia water, stir evenly and set aside. Place the mixed solution A in a magnetic stirring water bath, then prepare a micro peristaltic pump, connect the inlet and outlet hoses to solution B and fix them on the beaker mouth of solution A respectively, turn on the magnetic stirring to 500 rpm, set the water bath temperature to 40°C, and start the peristaltic pump at the same time, set the flow rate to 10 g / min, and slowly add solution B to the mixed solution A under stirring; finally, place the precipitate in the beaker in a 40°C water bath for aging for 12 hours, filter out the precipitate, rinse with deionized water and ethanol several times until the precipitate is neutral, dry the precipitate at 105°C to constant weight, and grind it for later use after drying. Weigh 20 g of the ground powder (100 mesh) into a hydrothermal reactor, add 1000 ml of deionized water (i.e., 1000 g of deionized water) thereto, stir evenly to obtain a suspension; adjust the pH of the suspension to 9.2 with ammonia water; seal the hydrothermal reactor, place it in a 190°C oven, and perform a hydrothermal reaction for 8 hours; after 8 hours, wait for the hydrothermal reactor to cool naturally to room temperature, filter out the product, rinse with deionized water and ethanol until neutral, and place the product in a 105°C oven to dry for 12 hours to obtain titanium dioxide composite hydroxyapatite.
[0108] Step 2: According to the mass ratio of styrene acrylic emulsion A (brand: Latex LX407S12) and acrylic emulsion B (brand: LatexLX854E) of 1.1:1, weigh and add them to a beaker, disperse them evenly with a disperser, pour them out for use, and mark the adhesive mixed emulsion C. Then, according to the mass ratio of TiO2 composite hydroxyapatite and deionized water of 0.45:1, weigh TiO2 composite hydroxyapatite and deionized water, add them to a closed drum ball mill, pour them out after ball milling for 8 hours, and mark TiO2 composite hydroxyapatite suspension D. Finally, mix emulsion C and suspension D at a mass ratio of 0.06:1 and set them aside. Prepare 1000g of spherical alumina and place it in a coating machine, set the rotation speed to 20r / min, and then use the atomization device of the coating machine to atomize 500g of the C+D mixed solution onto the surface of the spherical alumina. Finally, use the hot air device of the coating machine (set temperature 80°C) to dry and solidify the alumina surface to obtain nano-titanium dioxide composite hydroxyapatite photocatalytic material (TiO2 composite hydroxyapatite photocatalytic particles).
[0109] Among them, the solid content of styrene acrylic emulsion A is 40%, pH is 6, viscosity is 3000mPa.S, surface tension is 70mN / m, particle size is 80nm, and glass transition temperature is -100℃.
[0110] Acrylic emulsion B has a solid content of 45%, a pH of 6, a viscosity of 10 mPa.S, a surface tension of 30 mN / m, a particle size of 400 nm, and a glass transition temperature of 20°C.
[0111] The emulsion mixed with styrene acrylic emulsion A and acrylic emulsion B has a glass transition temperature range of -5°C.
[0112] Spherical alumina particle size: 1.0 mm, specific surface area 150 m / g 2 , water absorption ≥ 21%, crushing strength 150N, bulk density 0.4g / cm 3 .
[0113] Example 2
[0114] The difference between Example 2 and Example 1 is that the molar ratio of Ti / (Ca+Ti) is 0.5, and the other preparation methods are the same as those of Example 1.
[0115] Example 3
[0116] The difference between Example 3 and Example 1 is that the molar ratio of Ti / (Ca+Ti) is 0.7, and the other preparation methods are the same as those of Example 1.
[0117] Example 4
[0118] The difference between Example 4 and Example 1 is that the molar ratio of Ti / (Ca+Ti) is 0.9, and the other preparation methods are the same as those of Example 1.
[0119] Example 5
[0120] The difference between Example 5 and Example 1 is that the molar ratio of Ti / (Ca+Ti) is 0.05, and the other preparation methods are the same as those of Example 1.
[0121] Example 6
[0122] The difference between Example 6 and Example 1 is that the molar ratio of Ti / (Ca+Ti) is 1.0, and the other preparation methods are the same as those of Example 1.
[0123] Example 7
[0124] The difference between Example 7 and Example 1 is that the molar ratio of Ti / (Ca+Ti) is 3.0, and the other preparation methods are the same as those of Example 1.
[0125] Example 8
[0126] Step 1: According to the P / Ca molar ratio of 0.5, weigh calcium chloride and ammonium dihydrogen phosphate in a 1000mL beaker, add 250mL of deionized water to the beaker, prepare calcium chloride and ammonium dihydrogen phosphate solutions (solution B), stir until completely dissolved and set aside. Then, according to the molar ratio of Ti / (Ca+Ti) equal to 0.1, add titanium chloride solution to the calcium chloride solution under ice bath conditions, stir evenly and set aside (mixed solution A). Finally, adjust the mixed solution A and solution B to pH = 8.5 with ammonia water, stir evenly and set aside. Place the mixed solution A in a magnetic stirring water bath, then prepare a micro peristaltic pump, connect the inlet and outlet hoses to the solution B and fix them on the beaker mouth of the solution A respectively, turn on the magnetic stirring to 500 rpm, set the water bath temperature to 35°C, turn on the peristaltic pump at the same time, set the flow rate to 1g / min, and slowly add the solution B dropwise into the mixed solution A under stirring; finally, place the precipitate in the beaker in a 35°C water bath for aging for 24 hours, filter out the precipitate, rinse with deionized water and ethanol several times until the precipitate is neutral, dry the precipitate at 60°C to constant weight, and grind it for later use after drying. Weigh 10 g of the ground powder (40 mesh) into a hydrothermal reactor, add 1000 ml of deionized water (i.e., 1000 g of deionized water) thereto, stir evenly to obtain a suspension; adjust the pH of the suspension to 8.5 with ammonia water; seal the hydrothermal reactor, place it in an oven at 180°C, and perform a hydrothermal reaction for 24 hours; after 24 hours, wait for the hydrothermal reactor to cool naturally to room temperature, filter out the product, rinse with deionized water and ethanol until neutral, and place the product in an oven at 60°C to dry for 24 hours to obtain titanium dioxide composite hydroxyapatite.
[0127] Step 2: According to the mass ratio of styrene acrylic emulsion A (brand: Latex LX407S12) and acrylic emulsion B (brand: LatexLX854E) of 1.0:1, weigh and add them to a beaker, disperse them evenly with a disperser, pour them out for use, and mark the adhesive mixed emulsion C. Then, according to the mass ratio of TiO2 composite hydroxyapatite and deionized water of 0.30:1, weigh TiO2 composite hydroxyapatite and deionized water, add them to a closed drum ball mill, pour them out after ball milling for 24 hours, and mark TiO2 composite hydroxyapatite suspension D. Finally, mix emulsion C and suspension D at a mass ratio of 0.03:1 and set them aside. Prepare 1000g of spherical alumina and place it in a coating machine, set the rotation speed to 20r / min, and then use the atomization device of the coating machine to atomize 1200g of the C+D mixed solution onto the surface of the spherical alumina. Finally, use the hot air device of the coating machine (set temperature 60°C) to dry and solidify the alumina surface to obtain nano-titanium dioxide composite hydroxyapatite photocatalytic material (TiO2 composite hydroxyapatite photocatalytic particles).
[0128] Among them, the solid content of styrene acrylic emulsion A is 50%, pH is 9, viscosity is 20mPa.S, surface tension is 30mN / m, particle size is 200nm, and glass transition temperature is 50℃.
[0129] Acrylic emulsion B has a solid content of 50%, a pH of 9, a viscosity of 1000 mPa.S, a surface tension of 70 mN / m, a particle size of 100 nm, and a glass transition temperature of -40°C.
[0130] Emulsion mixed with styrene acrylic emulsion A and acrylic emulsion B, glass transition temperature range: 10℃.
[0131] Spherical alumina particle size: 5.0 mm, specific surface area 155 m / g 2 , water absorption ≥ 22%, crushing strength 155N, bulk density 0.9g / cm 3 .
[0132] Example 9
[0133] Step 1: According to the P / Ca molar ratio of 0.7, weigh calcium chloride and ammonium dihydrogen phosphate in a 1000mL beaker, add 250mL of deionized water to the beaker, prepare calcium chloride and ammonium dihydrogen phosphate solutions (solution B), stir until completely dissolved and set aside. Then, according to the molar ratio of Ti / (Ca+Ti) equal to 0.1, add titanium chloride solution to the calcium chloride solution under ice bath conditions, stir evenly and set aside (mixed solution A). Finally, adjust the mixed solution A and solution B to pH = 9.5 with ammonia water, stir evenly and set aside. Place the mixed solution A in a magnetic stirring water bath, then prepare a micro peristaltic pump, connect the inlet and outlet hoses to solution B and fix them on the beaker mouth of solution A respectively, turn on the magnetic stirring to 500 rpm, set the water bath temperature to 80°C, and start the peristaltic pump at the same time, set the flow rate to 50 g / min, and slowly add solution B to the mixed solution A under stirring; finally, place the precipitate in the beaker in an 80°C water bath for aging for 1 hour, filter out the precipitate, rinse with deionized water and ethanol several times until the precipitate is neutral, dry the precipitate at 150°C to constant weight, and grind it for later use after drying. Weigh 500g of the ground powder (400 mesh) into a hydrothermal reactor, add 1000ml of deionized water (i.e., 1000g of deionized water) thereto, stir evenly to obtain a suspension; adjust the pH of the suspension to 9.5 with ammonia water; seal the hydrothermal reactor, place it in a 250°C oven, and perform hydrothermal reaction for 4h; after 4h, wait for the hydrothermal reactor to cool naturally to room temperature, filter out the product, rinse with deionized water and ethanol until neutral, and place the product in a 150°C oven to dry for 4h to obtain titanium dioxide composite hydroxyapatite.
[0134] Step 2: According to the mass ratio of 10:1 of styrene acrylic emulsion A (brand: Latex LX407S12) and acrylic emulsion B (brand: LatexLX854E), weigh and add them to a beaker, disperse them evenly with a disperser, pour them out for use, and mark them as adhesive mixed emulsion C. Then, according to the mass ratio of TiO2 composite hydroxyapatite and deionized water of 0.90:1, weigh TiO2 composite hydroxyapatite and deionized water, add them to a closed drum ball mill, pour them out after ball milling for 4 hours, and mark them as TiO2 composite hydroxyapatite suspension D. Finally, mix emulsion C and suspension D at a mass ratio of 0.2:1 and set them aside. Prepare 1000g of spherical alumina and place it in a coating machine, set the rotation speed to 20r / min, and then use the atomization device of the coating machine to atomize 200g of the C+D mixed solution onto the surface of the spherical alumina. Finally, use the hot air device of the coating machine (set temperature 150°C) to dry and solidify the alumina surface to obtain nano-titanium dioxide composite hydroxyapatite photocatalytic material (TiO2 composite hydroxyapatite photocatalytic particles).
[0135] Among them, the solid content of styrene acrylic emulsion A is 45%, pH is 7, viscosity is 1000mPa.S, surface tension is 50mN / m, particle size is 100nm, and glass transition temperature is 0°C.
[0136] Acrylic emulsion B has a solid content of 48%, a pH of 7, a viscosity of 500 mPa.S, a surface tension of 40 mN / m, a particle size of 200 nm, and a glass transition temperature of 0°C.
[0137] Emulsion mixed with styrene acrylic emulsion A and acrylic emulsion B, glass transition temperature range: 0℃.
[0138] Spherical alumina particle size: 3.0 mm, specific surface area 150 m / g 2 , water absorption ≥ 21%, crushing strength 150N, bulk density 0.5g / cm 3 .
[0139] Comparative Example 1
[0140] Commercially available coconut shell activated carbon for cigarette filters, model: 6-12 mesh, link: Coconut shell activated carbon for cigarette filters removes tar, nicotine and other toxic and harmful substances in cigarettes (baidu.com).
[0141] Comparative Example 2
[0142] The Aiyisi purifier is equipped with AS-Sorb sterilizing filter media, which is advertised to remove smoke odor.
[0143] Comparative Example 3
[0144] The difference between Comparative Example 3 and Example 1 is that the molar ratio of Ti / (Ca+Ti) is 3.5, and the other preparation methods are the same as those of Example 1.
[0145] Comparative Example 4
[0146] The difference between Comparative Example 4 and Example 1 is that the molar ratio of Ti / (Ca+Ti) is 0.02, and the other preparation methods are the same as those of Example 1.
[0147] Comparative Example 5
[0148] The difference between Comparative Example 5 and Example 1 is that the molar ratio of P / Ca is 0.3, the dripping rate of solution B is 0.5 g / min, and the other preparation methods are the same as those of Example 1.
[0149] Comparative Example 6
[0150] The difference between Comparative Example 6 and Example 1 is that the molar ratio of P / Ca is 0.9, the dripping rate of solution B is 55 g / min, and the other preparation methods are the same as those of Example 1.
[0151] Comparative Example 7
[0152] The difference between Comparative Example 7 and Example 1 is that the molar ratio of P / Ca is 0.9, the dripping rate of solution B is 55 g / min, the static aging temperature is 30° C., and the other preparation methods are the same as those in Example 1.
[0153] Comparative Example 8
[0154] The difference between Comparative Example 8 and Example 1 is that the molar ratio of P / Ca is 0.3, the dripping rate of solution B is 0.5 g / min, the static aging temperature is 90° C., and the other preparation methods are the same as those in Example 1.
[0155] Comparative Example 9
[0156] The difference between Comparative Example 9 and Example 1 is that the molar ratio of P / Ca is 0.9, the dripping rate of solution B is 55 g / min, the static aging temperature is 30° C., the hydrothermal reaction temperature is 270° C., and the other preparation methods are the same as those in Example 1.
[0157] Comparative Example 10
[0158] The difference between Comparative Example 10 and Example 1 is that the molar ratio of P / Ca is 0.3, the dripping rate of solution B is 0.5 g / min, the static aging temperature is 90° C., the hydrothermal reaction temperature is 160° C., and the other preparation methods are the same as those in Example 1.
[0159] Experimental Example 1
[0160] Examples 1-7 and Comparative Examples 1-10 were respectively bonded to a plastic grid with a size of 386×330×5 mm and installed on an air purifier with a rated air volume of 500 CMH. The ultraviolet lamp of the purifier was turned on (wavelength 254 nm, the light source could fully cover the plastic grid), and the removal effects of cigarette odor and cigarette-related gaseous pollutants were tested with reference to the odor rating (as shown in Table 1) and test method of the national standard GB / T 18801-2022. The results are shown in Tables 2, 3 and 4.
[0161] Table 1 Odor rating table
[0162] Odor intensity Judgment content 0 Odorless 1 Seemingly existent 2 Slightly smelly 3 Obviously taste 4 Strong taste 5 Unbearable
[0163] Table 2 Cigarette odor removal
[0164]
[0165]
[0166] Table 3 Gaseous pollutant removal effect (30m 3 Warehouse / 8 hours)
[0167] Gaseous pollutants Acetaldehyde Ammonia Acetic acid TVOC Example 1 96% 90% 99% 93% Example 2 97% 92% 99% 96% Example 3 98% 94% 99% 97% Example 4 99% 98% 99% 99% Example 5 95% 90% 99% 93% Example 6 97% 95% 99% 97% Example 7 96% 91% 99% 93% Comparative Example 1 45% 65% 99% 99% Comparative Example 2 39% 73% 99% 99% Comparative Example 3 83% 82% 99% 90% Comparative Example 4 81% 84% 99% 90% Comparative Example 5 65% 88% 99% 86% Comparative Example 6 79% 80% 99% 56% Comparative Example 7 74% 81% 99% 73% Comparative Example 8 45% 78% 99% 86% Comparative Example 9 77% 84% 99% 54% Comparative Example 10 68% 80% 99% 77%
[0168] Table 4 Specific surface area comparison
[0169]
[0170]
[0171] According to the comparison of Table 2, Table 3 and Table 4, although Comparative Examples 1 and 2 have a higher specific surface area, they are not suitable for the subdivided field of cigarette purification. In the description of Examples 1-7, as the Ti composite ratio increases, the particle size of the titanium dioxide component in the composite material decreases. When the molar ratio of Ti / (Ca+Ti) is 0.9 (Example 4), the particle size of the titanium dioxide component in the composite material reaches the minimum value, while the particle size of hydroxyapatite reaches the maximum value; it shows that small particles of nano titanium dioxide can be dispersed on the surface of large particles of hydroxyapatite, and good dispersibility is obtained. At the same time, the specific surface area is also increased, and the cigarette-related purification indicators are also better.
[0172] However, the data of Examples 1-7 and Comparative Example 3 also show that the molar ratio of Ti / (Ca+Ti) cannot be increased indefinitely. When it exceeds the preferred ratio, the particle size of nano-titanium dioxide increases, while the particle size of hydroxyapatite fluctuates greatly, resulting in a decrease in the specific surface area of the material.
[0173] Experimental Example 2
[0174] Fourier transform infrared spectroscopy was performed on Examples 1-5, titanium dioxide and hydroxyapatite. The results are shown in Figure 2 ; Among them, a is Example 4, b is Example 3, c is Example 2, d is Example 1, e is pure TiO2, and f is pure hydroxyapatite.
[0175] according to Figure 2 It can be seen from Figure 5 that pure TiO2 powder has a wavelength of 800-450cm -1 The broad absorption peak at is the stretching vibration peak of the Ti-O bond. Figure 2 From f, we can see that pure hydroxyapatite is at 962cm -1 and 602cm -1 The absorption peaks at 1091 cm-1 are the stretching vibration peaks of the PO bond and the triple degenerate vibration peaks in PO4(3-). The stretching vibration peak of POH appears at 1091 cm-1. -1 and 632cm -1 The above absorption peaks indicate the presence of HPO4(2-) in hydroxyapatite.
[0176] Figure 2 a, b, c, and d are FTIR spectra of TiO2 / hydroxyapatite composite nanomaterials with different Ti / (Ca+Ti) molar ratios. Figure 2 From a, b, c, and d, we can see that the characteristic absorption peak of hydroxyapatite appears at 566 cm -1 、602cm -1 、632cm -1 、962cm -1 、1033cm -1 、1091cm -1 It indicates that hydroxyapatite exists in the composite nanomaterial; since the characteristic peak of TiO2 appears in the range of 800-450cm -1 Therefore, from the shape of the peak, it can be judged that the TiO2 in the composite material mainly exists in the anatase crystal form.
[0177] Experimental Example 3
[0178] Nicotine with a relatively high concentration in cigarette smoke and 3-vinylpiperidine, a nicotine pyrolysis product, were used as characterizing substances to compare the effects of turning on and off the UVC lamp to Example 4 and various comparative examples. The data are shown in Table 5.
[0179] Table 5 Decomposition effect of nicotine and 3-vinylpiperidine
[0180]
[0181]
[0182] The data in Table 5 show that Comparative Example 1 has basically no purification effect on 3-vinylpiperidine. After turning on the UVC lamp, Comparative Example 1 still has no improvement in the adsorption of nicotine, indicating that the purification effect is only due to the adsorption of the material itself, and there is no actual decomposition effect. The data in Example 4 show that ultraviolet light can effectively increase the decomposition rate of nicotine and 3-vinylpiperidine by the composite material.
[0183] The data of comparative examples 3-10 show that the material has basically no purification effect on 3-vinylpiperidine. After turning on the UVC lamp, there is still no improvement. Under the condition of turning off the UVC lamp, the material has a certain adsorption effect on nicotine, and after turning on the UVC lamp, the nicotine adsorption performance has not been improved, indicating that nicotine is physically adsorbed entirely by the specific surface area of the material itself, and there is no actual photodecomposition effect. This may be due to the difference in process conditions during the synthesis process, resulting in the titanium dioxide particle size being too large (≥40nm), and the large particle size mainly affects the photocatalytic performance in the following ways: ① The larger the particle size, the smaller the surface area; the surface area is the main place where the photocatalytic reaction occurs, and the reduction in surface area will lead to a decrease in the reaction rate, thereby affecting the performance of the photocatalyst. ② The light absorption capacity of titanium dioxide is related to its particle size. The larger the particle size, the weaker the light absorption capacity; the weakened light absorption capacity will lead to a decrease in the photocatalytic reaction rate. ③ When the particle size is too large, the recombination rate of electron-hole pairs will increase, thereby reducing the efficiency of the photocatalytic reaction. ④ When the particle size is too large, the aggregation phenomenon between particles will be aggravated, resulting in a reduction in the contact area between particles, which in turn affects the efficiency of the photocatalytic reaction.
[0184] Experimental Example 4
[0185] The photocatalytic material of Example 4 was white before being used to absorb tar, and the photocatalytic material of Example 4 after absorbing tar was yellow-brown; the photocatalytic material of Example 4 after absorbing tar was irradiated with UVC light, and the color difference between the photocatalyst of Example 4 after loading tar and that of Example 4 not used for absorbing tar was continuously monitored, represented by ΔE, and the trend was shown in FIG. Figure 3 The data show that as the irradiation time increases, the color difference between the two becomes smaller and smaller, indicating that the photocatalyst of Example 4 continues to decompose the tobacco tar after adsorption.
[0186] Experimental Example 5
[0187] Example 4 and Comparative Examples 1-10 were respectively bonded to a plastic grid with a size of 386×330×5 mm and installed on an air purifier with a rated air volume of 500 CMH. The ultraviolet lamp of the purifier was turned on (wavelength 254 nm, the light source could fully cover the plastic grid), and then cigarettes were continuously loaded. Referring to the odor rating of the national standard GB / T 18801-2022 (as shown in Table 1), the odor changes at the air outlet of the air purifier were regularly monitored. The results are shown in Table 6.
[0188] Table 6 Rating of odor at the air outlet after continuous cigarette loading
[0189]
[0190] Comparative Examples 1 and 2 show that the higher specific surface area has a certain adsorption effect on the smoke smell, but as the adsorption is saturated, Comparative Example 2 first breaks through 3 points, and the score rises all the way, and after loading 75 cigarettes, the smell of Comparative Example 1 also breaks through 3 points, indicating that the adsorption is also saturated. In Example 4, the smell of cigarettes is still maintained below 2.5 points after long-term loading, and no secondary odor is generated, indicating that the smoke tar intercepted in Example 4 is fully decomposed.
[0191] The data of comparative examples 3-10 show that after loading 25 cigarettes, most of the odors can basically be maintained below 3 points, and after loading 50 cigarettes, the odor scores all exceed 3 points. As the number of loaded cigarettes increases, the odor scores rise rapidly and finally reach a maximum value of 5 points, indicating that the comparative example has no significant effect in decomposing tobacco tar, which is consistent with the decomposition effect of nicotine and 3-vinylpiperidine in Table 5.
[0192] Experimental Example 6
[0193] The antibacterial property of Example 4 was tested with reference to GB 21551-2010. The data showed that Example 4 had excellent antibacterial property. The data are shown in Table 7:
[0194] Table 7 Antibacterial rate of accessories
[0195]
[0196] Experimental Example 7
[0197] Examples 1-4 and comparative examples 3-10 were fixed on the workbench of the ultraviolet irradiation equipment, and the irradiation time was set to 200 hours. During the irradiation process, the surface condition and color change of the samples were recorded every 50 hours. The data showed that the materials of Examples 1-4 still maintained excellent hardness and stable color appearance after long-term ultraviolet irradiation. The results are shown in Table 8.
[0198] Table-8 Comparison of UV resistance of materials
[0199]
[0200]
[0201] In summary, the photocatalytic material of nano-titanium dioxide composite hydroxyapatite prepared by the preparation method of the present invention can effectively decompose tobacco tar and nicotine under the action of photocatalysis, decomposing them into volatile, odorless substances, thereby improving the secondary pollution problem caused by the desorption of tobacco tar and improving the air purification effect; moreover, the photocatalytic material of nano-titanium dioxide composite hydroxyapatite also has good antibacterial, anti-ultraviolet and long-lasting photocatalytic properties.
[0202] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a photocatalytic material of nano-titanium dioxide composite hydroxyapatite, characterized in that: include: At a first preset temperature and under stirring conditions, adding a diammonium phosphate solution dropwise to a mixed solution of calcium chloride and titanium chloride to obtain a first precipitate; The first precipitate is allowed to stand for aging at a second preset temperature, and then filtered to obtain a first filtrate; The first filtrate is washed to neutrality, and then dried and ground; The ground first filtrate is subjected to a hydrothermal reaction at a third preset temperature, filtered, and washed to obtain titanium dioxide composite hydroxyapatite; Mixing the titanium dioxide composite hydroxyapatite suspension and the emulsion to obtain a suspension; The suspension is made to adhere to the surface of the porous material particles and dried to solidify.
2. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: The Ti / (Ca+Ti) ratio in the mixed solution of the calcium chloride and the titanium chloride is 0.05 to 3.0; and / or, The molar ratio of P in the ammonium dihydrogen phosphate solution to Ca in the mixed solution of calcium chloride and titanium chloride is 0.5 to 0.
7.
3. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: The diammonium phosphate solution is added dropwise to the mixed solution of the calcium chloride and the titanium chloride at a dripping rate of 1.0 to 50 g / min.
4. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: The pH of the diammonium phosphate solution and the mixed solution of the calcium chloride and the titanium chloride is 8.5-9.5; and / or, The first preset temperature is 35-80° C.; and / or, The second preset temperature is 35-80° C.; and / or, The static aging time is 1 to 24 hours; and / or, The temperature of the first filtrate which is dried, cleaned and neutralized is 60-150° C.; and / or, The mesh size of the first filtrate after grinding is 40 to 400 meshes.
5. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: The first filtrate after grinding is mixed with water to carry out the hydrothermal reaction, wherein the mass ratio of the first filtrate after grinding to water is (0.01-0.5):1; and / or, The pH of the first filtrate after grinding during the hydrothermal reaction is 8.5 to 9.5; and / or, The third preset temperature is 180-250° C.; and / or, The reaction time of the hydrothermal reaction is 4 to 24 hours; and / or, After the hydrothermal reaction, filtration and washing, the titanium dioxide composite hydroxyapatite is obtained by drying at a temperature of 60 to 150° C. for 4 to 24 hours.
6. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: The emulsion comprises a styrene-acrylic emulsion and an acrylic emulsion, wherein the mass ratio of the styrene-acrylic emulsion to the acrylic emulsion is (1-10):1, and the glass transition temperature of the emulsion is -5-10°C; and / or, The mass ratio of the emulsion to the suspension of titanium dioxide-composite hydroxyapatite is (0.03-0.2):1; and / or, The preparation method of the titanium dioxide composite hydroxyapatite suspension comprises: mixing the titanium dioxide composite hydroxyapatite and water at a mass ratio of (0.3-0.9):1 by ball milling.
7. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 6, characterized in that: The styrene-acrylic emulsion has a solid content of 40-50%, a pH of 6-11, a viscosity of 20-3000 mPa.S, a surface tension of 30-70 mN / m, a particle size of 80-200 nm, and a glass transition temperature of -100-50°C; and / or, The acrylic emulsion has a solid content of 45-50%, a pH of 6-9, a viscosity of 10-1000 mPa.S, a surface tension of 30-70 mN / m, a particle size of 100-400 nm, and a glass transition temperature of -40-20°C.
8. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: The mass ratio of the suspension to the porous material particles is (0.2-1.2):
1.
9. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: The porous material particles include at least one of aluminum oxide particles, activated carbon particles, molecular sieve particles and silica gel particles.
10. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: The porous material particles have a particle size of 1.0-5.0 mm and a specific surface area of ≥150 m / g 2 , water absorption ≥ 21%, crushing strength ≥ 150N, bulk density 0.4~0.9g / cm 3 .
11. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: After the suspension is attached to the surface of the porous material particles, the drying temperature is 60-150°C.
12. The method for preparing the photocatalytic material of nano-titanium dioxide composite hydroxyapatite according to claim 1, characterized in that: The method for attaching the suspension to the porous material particles comprises: stirring the porous material particles at a rotation speed of 15-25 r / min, and then atomizing and spraying the suspension onto the surface of the porous material particles.
13. A photocatalytic material of nano-titanium dioxide composite hydroxyapatite, characterized in that: The photocatalytic material is prepared by the method for preparing the nano titanium dioxide composite hydroxyapatite photocatalytic material according to any one of claims 1 to 12.
14. A photodegradable smoke tar filter, characterized in that: include: A HEPA layer, an activated carbon layer and an LED substrate layer are stacked, and the photocatalytic material of nano-titanium dioxide composite hydroxyapatite as claimed in claim 13 is attached to the HEPA layer and / or the activated carbon layer.
15. The photodegradable smoke tar filter according to claim 14, characterized in that: The HEPA layer includes a PET layer stacked in sequence with the photocatalytic material loaded with the nano-titanium dioxide composite hydroxyapatite, an intermediate layer formed by melt-blowing the PP masterbatch of the photocatalytic material attached with the nano-titanium dioxide composite hydroxyapatite, the hindered amine PP masterbatch, and the PP masterbatch blended and melt-blown, and a hindered amine-modified PP non-woven fabric layer; wherein the side of the PET layer facing away from the intermediate layer is the air inlet side.
16. The photodegradable smoke tar filter according to claim 14, characterized in that: The activated carbon layer comprises a hindered amine-modified PP plastic grid layer and a columnar activated carbon layer modified by the photocatalytic material of the nano-titanium dioxide composite hydroxyapatite, which are stacked in sequence.
17. The photodegradable smoke tar filter according to claim 14, characterized in that: The LED substrate layer includes a high thermal conductivity aluminum nitride substrate and UVC-LED lamp beads. The high thermal conductivity aluminum nitride substrate has multiple assembly areas, which are respectively distributed in different areas of the high thermal conductivity aluminum nitride substrate, and the assembly areas are provided with assembly holes, and the UVC-LED lamp beads are assembled in the assembly holes.
Citation Information
Patent Citations
Photocatalytic air purification device based on diffused optical fibers
CN103463971A
Waste gas treatment system of synthetic leather three-plate printing machine
CN115738695A
Method for preparing TiO2 / titanium supported hydroxyapatite complex phase absorption and disinfection nano material
CN1701845A
Office uses air purification device
CN207487034U
Vehicle-mounted photocatalytic oxidation deodorization device
CN210674685U