Hydrodeoxygenation catalyst for biological aviation oil precursor, preparation method and application
By using catalysts supported by zirconium phosphate with Nb2O5 and hydrogenation active metals in the preparation of bioaero oil, the problems of insufficient catalytic performance and single product in the prior art are solved, and the rich components of bioaero oil are efficiently prepared and the products are improved Mass and catalyst stability.
Patent Information
- Application Number
- CN202411175992.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing hydrodeoxygenation catalysts have problems such as insufficient catalytic performance, single product components, and easy deactivation of the catalyst in the preparation of bioaerospace. In particular, the loading of non-precious metal catalysts is high and the particles are large, resulting in low preparation efficiency.
Using a catalyst supported by zirconium phosphate with Nb2O5 and hydrogenation active metal, high-dispersed nano-sized metal particles were prepared by hydrothermal method, combined with the synchronous addition of zirconium phosphate support and metal salt, and using low-carbon diol chelation to inhibit metal agglomeration, it was prepared. A catalyst with high hydrothermal stability.
The high yield and abundant product distribution of bioaero oil components are achieved, the yield and quality of the product are improved, and the stability and efficiency of the catalyst are improved.
Smart Images

Figure CN119056475A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomass liquid fuel, and in particular relates to a catalyst for hydrogenation and deoxygenation of a bio-jet fuel precursor, a preparation method and an application thereof. Background Art
[0002] Sustainable aviation fuel has become one of the most concerned issues in the world today. As a renewable organic carbon source, lignocellulosic biomass is abundant on Earth. Using lignocellulosic biomass as a raw material to obtain renewable bio-aviation fuel (SAF) is expected to reduce carbon emissions from the aviation industry by 55%-92%.
[0003] Invention patents CN103450940A, CN104119943A, CN103805224A, CN105779036A, etc. involve the synthesis of long carbon chain oxygen-containing compounds by base-catalyzed aldol condensation reaction of wood fiber-based furfural compounds (furfural, methyl furfural, hydroxymethyl furfural) and ketones (methyl isobutyl ketone, mesityl oxide, levulinic acid, etc.), and the long carbon chain oxygen-containing compounds are then subjected to hydrogenation deoxygenation reaction to obtain a series of long chain hydrocarbon compounds. Among them, the hydrogenation deoxygenation catalysts are all bifunctional catalysts of hydrogenation active metals Pd, Pt, Ru, Ir, Ni coupled with solid acids such as alumina and molecular sieves. This metal-acid bifunctional catalyst with solid acid as carrier and responsible for hydrogenation of active metal has good hydrodeoxygenation effect, especially precious metal catalyst, which has a high alkane yield. However, there are still many problems with existing catalysts, such as: only effective for hydrodeoxygenation reaction, unable to complete carbon chain isomerization, cyclization and other reactions at the same time, and the product components are relatively single; water produced by hydrodeoxygenation is corrosive to catalytic materials such as alumina and molecular sieves in a high temperature environment, and the catalyst is easily deactivated; non-precious metal catalysts have high loading and large particles, and the catalytic performance is insufficient. Therefore, it is urgent to develop new hydrodeoxygenation refining catalysts to achieve efficient preparation of bio-jet fuel. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a catalyst for the hydrodeoxygenation of bio-jet fuel precursors, a preparation method and an application thereof, thereby solving the problems in the prior art.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] The preparation method of a catalyst for hydrodeoxygenation of a bio-jet fuel precursor comprises the following steps:
[0007] S1, dissolving ZrOCl2 and (NH4)2HPO4 in water respectively, mixing the two solutions under stirring, adding ammonia water dropwise, and placing the obtained solid mixture in an autoclave after sufficient stirring, and heating at a temperature of 100°C; then filtering, washing, drying, and calcining to obtain a zirconium phosphate carrier;
[0008] S2, dissolving the metal salt and NbCl5 in water at the same time, then adding a low-carbon diol and stirring evenly; ultrasonically dispersing the zirconium phosphate carrier in the solution, evaporating the water under stirring conditions, and then drying, calcining, and reducing in a hydrogen atmosphere to obtain a zirconium phosphate catalyst loaded with metal and NbCl5.
[0009] Furthermore, the loading amount of NbCl5 in the catalyst is 5-20%, and the loading amount of metal is 1-30%.
[0010] Furthermore, the metal salt is one or two of Pd, Pt, Ru, Ni, Fe, and Cu metal salts.
[0011] Furthermore, in the zirconium phosphate carrier, the molar ratio of ZrOCl2 to (NH4)2HPO4 is 1:0.2-2.5.
[0012] Furthermore, the low-carbon diol is ethylene glycol or propylene glycol.
[0013] Furthermore, in S1, the heat preservation and heating conditions are: maintaining at 100°C for 24 hours; and the calcination temperature of the zirconium phosphate carrier is 400-600°C.
[0014] Furthermore, in S2, the calcination temperature is 300-350°C, and the reduction temperature is 400-450°C.
[0015] A catalyst for the hydrodeoxygenation of a bio-jet fuel precursor is prepared using the above-mentioned method for preparing the catalyst for the hydrodeoxygenation of a bio-jet fuel precursor.
[0016] The above-mentioned bio-jet fuel precursor hydrodeoxygenation catalyst is used in the preparation of bio-jet fuel components.
[0017] Furthermore, the application includes: taking the bio-jet fuel precursor as a raw material, carrying out a hydrodeoxygenation conversion under the action of the hydrodeoxygenation catalyst, and obtaining the bio-jet fuel component by catalyzing the double bond hydrogenation, furan ring opening, catalytic cracking, furan ring carbon chain rearrangement and cyclization, hydroxyl dehydration, carboxyl removal, and carbon chain isomerization reaction of the bio-jet fuel precursor molecule.
[0018] Beneficial effects of the present invention:
[0019] 1. The present invention proposes a hydrodeoxygenation catalyst of zirconium phosphate loaded with Nb2O5 and hydrogenation active metals for use in the bio-jet fuel refining process. The catalyst has the following advantages: First, niobium pentachloride is hydrolyzed to form hydrated niobium hydroxide precipitation when dissolved in water, and then the mesoporous carrier material zirconium phosphate is added, and the hydrated niobium hydroxide precipitation can be more evenly dispersed on the surface and in the pores of the carrier, which is conducive to the good interaction between the niobium oxide formed after roasting and the carrier; second, the metal salt and niobium pentachloride are added to the water simultaneously, and the metal salt can be well dispersed in the hydrated niobium hydroxide precipitation formed by hydrolysis, and at the same time, the metal ions are chelated and anchored with low-carbon diols to inhibit the agglomeration of metal ions during the roasting process, so as to achieve the efficient preparation of highly dispersed nano-scale metal particles.
[0020] 2. The components of the catalyst proposed in the present invention have high hydrothermal stability, the preparation conditions are easy to control, the method is simple, and the hydrocarbon yield of the product of catalytic hydrodeoxygenation of bio-jet fuel precursor is high and the composition is relatively rich, which is beneficial to improving the yield and quality of bio-jet fuel products. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0022] Figure 1 XRD pattern of Pd(5)-Nb2O5(10) / ZrP catalyst;
[0023] Figure 2 High-resolution transmission electron microscopy and EDS elemental analysis of Pd(5)-Nb2O5(10) / ZrP catalyst;
[0024] Figure 3 NH3-TPD curve of Pd(5)-Nb2O5(10) / ZrP catalyst;
[0025] Figure 4 Structural formula of the hydrodeoxygenation product of aviation fuel precursor catalyzed by Pd(5)-Nb2O5(10) / ZrP. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] In this example, a hydrodeoxygenation catalyst Pd(5)-Cu(10)-Nb2O5(5) / ZrP was prepared, wherein the mass fraction of Pd was 5%, the mass fraction of copper was 10%, and the mass fraction of Nb2O5 was 5%, that is, "(x)" represents the mass fraction, the same below, and the preparation method is as follows:
[0029] (1) First, 5.75 g of (NH4)2HPO4 was dissolved in 20 ml of deionized water, and 6.45 g of ZrOCl2 was dissolved in 40 ml of deionized water. The two prepared solutions were slowly mixed under vigorous stirring and ammonia water was added dropwise. The obtained white precipitate was further stirred;
[0030] (2) The solid mixture obtained after sufficient stirring is placed in a 100 ml high pressure autoclave and maintained at 100° C. for 24 h; the obtained solid sample is filtered, washed, dried, and then calcined at 500° C. for 2 h to obtain a zirconium phosphate carrier ZrP with an atomic ratio of P / Zr=2.5.
[0031] (3) 0.416 g PdCl2, 0.3575 g NbCl5 and 1.888 g Cu(NO3)2·3H2O were dissolved in deionized water, and a low-carbon diol was added dropwise. Then, 4.3925 g ZrP carrier was added, and the mixture was dispersed evenly by ultrasonication. The water was evaporated under stirring, and then the mixture was dried in an oven overnight. The dried sample was placed in a muffle furnace and calcined at 300°C for 3 hours. Finally, the sample was reduced at 400°C in a H2 atmosphere for 3 hours to obtain a Pd(5)-Cu(10)-Nb2O5(5) / ZrP catalyst, wherein the Cu loading was 10%, the Pd loading was 5%, and the Nb2O5 loading was 5%.
[0032] Example 2-Example 9
[0033] The preparation methods of the catalysts of Examples 2 to 9 are the same as those of Example 1, except that a series of catalysts were prepared by changing the P / Zr molar ratio of the carrier, the carrier calcination temperature, the type and content of the metal salt, the calcination temperature and the reduction temperature, as shown in Table 1.
[0034] Table 1 Catalyst loading and preparation conditions of Examples 2 to 9
[0035]
[0036] Among them, the Pd(5)-Nb2O5(10) / ZrP catalyst prepared in Example 3 was subjected to a series of characterizations, such as Figure 1As shown in the XRD test results, only obvious ZrP characteristic peaks were observed on the XRD curve, but no obvious Pd characteristic peaks were observed, indicating that the metal Pd was highly dispersed; no crystal characteristic peaks of Nb2O5 were observed in the XRD graph, only amorphous diffuse peaks were observed, indicating that Nb2O5 exists in an amorphous state, which is of great significance for promoting metal dispersion. Figure 2 (a) and (b) are the high-resolution transmission electron microscopy image and EDS surface scanning image of the Pd(5)-Nb2O5(10) / ZrP catalyst, respectively, which further confirm the highly dispersed and uniform distribution state of metal Pd and Nb2O5.
[0037] Figure 3 The acidity of the Pd(5)-Nb2O5(10) / ZrP catalyst was characterized by NH3-TPD technology. The NH3-TPD curve shows that the catalyst contains three acid centers of oxygen weak acid, medium strong acid and strong acid, with medium strong acid and strong acid centers being the main ones. The rich acid centers have a positive effect on the catalyst in promoting furan ring opening, carbon chain rearrangement, catalytic cracking and dehydration reactions.
[0038] Example 10
[0039] In this example, a 100 ml stainless steel high-pressure reactor was used to conduct an experimental study on the hydrodeoxygenation of the catalyst to produce aviation fuel components. The specific experimental process is as follows: 30 ml of cyclohexane, 0.6 g of C15 oxygen-containing precursor and 0.4 g of catalyst were added to the stainless steel reactor; after replacing the air in the reactor, the reactor was filled with H2 to the required pressure, and then heated to the required reaction temperature at a stirring speed of 600 rpm, and maintained for the preset reaction time. After the reaction was completed, the reactor was cooled to room temperature and samples were collected for analysis.
[0040] It is worth mentioning that the bio-jet fuel precursor is prepared by the aldol condensation of furfural and levulinic acid, and at least includes a mixture of a 1:1 condensation product of furfural and levulinic acid (A) and a 1:2 condensation product of furfural and levulinic acid (B);
[0041] The catalyst used in this example is Pd(5)-Nb2O5(10) / ZrP, the reaction temperature is 260°C, the reaction time is 12 hours, the hydrogen pressure is 5MPa, and the carbon yield of the hydrocarbon product is 85.5%. The main components of the product include branched alkanes, straight-chain hydrocarbons, and cycloalkanes, as shown in Table 2 and Table 3. Figure 4 shown.
[0042] Table 2 Composition of the products of hydrodeoxygenation of aviation fuel precursor catalyzed by Pd(5)-Nb2O5(10) / ZrP
[0043]
[0044]
[0045] Figure 2 The alkane products in the figure indicate the occurrence of furan ring opening reaction, hydrogenation saturation reaction of C=C and C=O, and dehydration reaction. The C9 and C14 hydrocarbon products in the figure indicate the occurrence of decarboxylation reaction, the C8, C11, C12, C13 and other hydrocarbon products indicate the occurrence of cracking reaction, the C8 and C9 branched hydrocarbon products indicate the occurrence of furan ring rearrangement reaction, and the branched hydrocarbon products indicate the occurrence of carbon chain isomerization reaction. These reactions occur under the synergistic effect of the acid center of the catalyst and the active metal.
[0046] Example 11-Example 21
[0047] The experimental process in Examples 11 to 21 differs from that in Example 10 only in that the catalyst type, hydrogen pressure, reaction temperature, and reaction time parameters are changed to carry out the hydrodeoxygenation experiment of the bio-jet fuel precursor. The experimental results are shown in Table 3.
[0048] Table 3 Effects of different catalysts and reaction conditions on the hydrodeoxygenation conversion of oxygen-containing precursors
[0049]
[0050] Comparative Example 1-Comparative Example 2
[0051] In Comparative Example 1 and Comparative Example 2, the catalysts are Pd-based catalysts prepared by impregnation method using Nb2O5 and ZrP as carriers, respectively. Specific experimental parameters and experimental results are shown in Table 4.
[0052] Table 4 Effect of using Pd-based catalyst on hydrodeoxygenation conversion of oxygen-containing precursors in comparative examples
[0053]
[0054] Combining Table 3 and Table 4, it can be seen that, except for the Fe-doped catalyst (Example 15), the catalysts prepared by the present invention have excellent catalytic performance, and even the base metal Ni catalyst has a hydrocarbon product yield of 80.3% (Example 14), which has great application prospects. In contrast, the catalysts prepared by using a single solid acid Nb2O5 or ZrP as a carrier in the comparative example have a low hydrocarbon product yield even if the precious metal Pd is loaded.
[0055] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0056] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A method for preparing a catalyst for hydrodeoxygenation of a bio-jet fuel precursor, characterized in that: The following steps are involved: S1, dissolving ZrOCl2 and (NH4)2HPO4 in water respectively, mixing the two solutions under stirring, adding ammonia water dropwise, and placing the obtained solid mixture in an autoclave after sufficient stirring, and heating at a temperature of 100°C; then filtering, washing, drying, and calcining to obtain a zirconium phosphate carrier; S2, dissolving the metal salt and NbCl5 in water at the same time, then adding a low-carbon diol and stirring evenly; ultrasonically dispersing the zirconium phosphate carrier in the solution, evaporating the water under stirring conditions, and then drying, calcining, and reducing in a hydrogen atmosphere to obtain a zirconium phosphate catalyst loaded with metal and NbCl5.
2. The method for preparing a bio-jet fuel precursor hydrodeoxygenation catalyst according to claim 1, characterized in that: The loading amount of NbCl5 in the catalyst is 5-20%, and the loading amount of metal is 1-30%.
3. The method for preparing a bio-jet fuel precursor hydrodeoxygenation catalyst according to claim 1, characterized in that: The metal salt is one or two of Pd, Pt, Ru, Ni, Fe, and Cu metal salts.
4. The catalyst for hydrodeoxygenation of bio-jet fuel precursor according to claim 1, characterized in that: In the zirconium phosphate carrier, the molar ratio of ZrOCl2 to (NH4)2HPO4 is 1:0.2-2.
5.
5. The method for preparing a bio-jet fuel precursor hydrodeoxygenation catalyst according to claim 1, characterized in that: The low carbon diol is ethylene glycol or propylene glycol.
6. The method for preparing a bio-jet fuel precursor hydrodeoxygenation catalyst according to claim 1, characterized in that: In S1, the heat preservation and heating conditions are: maintaining at 100°C for 24 hours; the calcination temperature of the zirconium phosphate carrier is 400-600°C.
7. The method for preparing a bio-jet fuel precursor hydrodeoxygenation catalyst according to claim 1, characterized in that: In S2, the calcination temperature is 300-350°C, and the reduction temperature is 400-450°C.
8. A catalyst for hydrodeoxygenation of bio-jet fuel precursor, characterized in that: The catalyst is prepared by using the method for preparing a bio-jet fuel precursor hydrodeoxygenation catalyst as described in any one of claims 1 to 7.
9. Use of the bio-jet fuel precursor hydrodeoxygenation catalyst according to claim 8 in the preparation of bio-jet fuel components.
10. The use according to claim 9, characterized in that: The application includes: taking the bio-jet fuel precursor as a raw material, carrying out a hydrodeoxygenation conversion under the action of the hydrodeoxygenation catalyst, and obtaining the bio-jet fuel component by catalyzing the double bond hydrogenation, furan ring opening, catalytic cracking, furan ring carbon chain rearrangement and cyclization, hydroxyl dehydration, carboxyl removal, and carbon chain isomerization reaction of the bio-jet fuel precursor molecule.
Citation Information
Patent Citations
Method for preparation of aviation kerosene and diesel oil from biomass derivative
CN103450940A
Preparation method for aviation kerosene
CN103805224A
Method for preparing aviation kerosene from furyl oxygen-containing organic compounds by hydrogenation deoxidation
CN104119943A
Method for producing oil for traffic fuel by using straws
CN105779036A
Preparation method of bio-based aviation fuel hydrofining catalyst
CN114669323A