Catalytic cracking catalyst as well as preparation method and application thereof
By introducing silicon source stabilizer and specific binder precursors during the catalyst preparation process and performing water vapor treatment, the problem of reduced activity of the catalyst under high temperature hydrothermal conditions and insufficient anti-metal pollution ability is solved, achieving high efficiency Heavy oil conversion and treatment of multiple metal contaminants.
Patent Information
- Application Number
- CN202310624125.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing metal-resistant catalytic cracking catalysts have decreased activity and stability under high temperature hydrothermal conditions, and their heavy oil conversion and metal pollution resistance are insufficient, especially in heavy metal deposition.
Using a catalytic cracking catalyst preparation method, a first suspension is formed by mixing the soluble compounds of the first binder precursor, the liquid medium and the silicon source stabilizer, and then with the cracking active components, clay and The second binder precursor is mixed, spray-dried to form particulate microspheres, and water vapor treatment is carried out at 100-500°C to produce a catalyst with excellent heavy oil conversion ability and anti-metal contamination ability.
The heavy oil conversion rate and total liquid product yield of the catalyst are improved, the resistance to metal pollution such as iron, vanadium, and nickel is enhanced, and catalytic activity and hydrothermal stability are significantly improved.
Smart Images

Figure BDA0004256383830000151 
Figure BDA0004256383830000161 
Figure BDA0004256383830000171
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalytic cracking catalyst preparation, and in particular to a catalytic cracking catalyst and a preparation method and application thereof. Background Art
[0002] With the increasing shortage of oil resources and the continuous rise in crude oil prices, major refineries have reduced costs by deeply processing heavy oil and using inferior oil to maximize benefits. Currently, catalytic cracking is an important means of heavy oil processing.
[0003] The catalytic cracking catalyst is the core of the process. It is mainly composed of molecular sieves and matrix, and the main components are silicon oxide and aluminum oxide. In general, the silicon and aluminum components are very stable, but under the high temperature and hydrothermal conditions of the regenerator, the interaction between the elements and water will cause a series of complex physical and chemical changes, which will lead to a decrease in catalyst activity and stability, a decrease in heavy oil conversion capacity, and poor product selectivity. At the same time, as the proportion of inferior raw materials increases, heavy metals such as nickel, vanadium, and iron brought by the raw materials will be deposited on the surface of the catalyst, causing the catalyst surface to sinter, forming a 2-3μm thick dense layer on the surface, blocking the channels for reactants to enter the catalyst and for product diffusion, further deteriorating product distribution.
[0004] US3944482 discloses a catalyst matrix with an average pore size of >9nm, which reduces the dispersion of heavy metal nickel and enhances the catalyst's nickel resistance. US4750988 discloses a vanadium trapping agent with MgO as the vanadium trapping active substance (mass fraction of 5% to 35%) and a specific surface area of 100 to 500m 2 / g, the proportion of the vanadium scavenger in the system is 10% to 15%, A12O3 is used as a carrier, n(MgO):n(A12O3)=(0.01-2):1, the optimal range is (0.05-0.5):1, and the mixed system can also contain 0.1% to 2% of vanadium oxide. The vanadium scavenger is made by impregnating magnesium compounds into A12O3, drying and roasting, which can improve the conversion rate and selectivity of the feed and increase the gasoline yield.
[0005] In general, the metal-resistant catalytic cracking catalysts currently reported for industrial applications are mainly composed of active components such as alumina, rare earths, and alkaline earth metals. These active components react with nickel and vanadium to generate more stable compounds, thereby achieving the effect of resistance to nickel and vanadium. Summary of the invention
[0006] The purpose of the present invention is to overcome the problem that the metal pollution resistance of existing metal-resistant catalytic cracking catalysts needs to be further improved, and to provide a catalytic cracking catalyst and its preparation method and application. The catalytic cracking catalyst prepared by the preparation method provided by the present invention has excellent heavy oil conversion ability and metal pollution resistance.
[0007] In order to achieve the above object, the present invention provides a method for preparing a catalytic cracking catalyst, which comprises the following steps:
[0008] (1) performing a first mixing of a first binder precursor, a liquid medium, and a soluble compound of a silicon source stabilizer to obtain a first suspension, wherein the viscosity of the first suspension is not less than 10000 mPa·s;
[0009] (2) performing a second mixing of the first suspension with a cracking active component containing a Y molecular sieve, clay, and a second binder precursor to obtain a second suspension;
[0010] (3) spray drying the second suspension to obtain particle microspheres;
[0011] (4) treating the microspheres with steam at 100-500° C. to obtain a catalytic cracking catalyst;
[0012] Wherein, the soluble compound of the silicon source stabilizer is a soluble compound of a transition metal element;
[0013] The amount of the soluble compound of the silicon source stabilizer is such that in the prepared catalyst, the silicon source stabilizer accounts for 0.1-10% by weight of the dry basis of the catalyst, wherein the silicon source stabilizer is calculated as oxide.
[0014] The inventors found in their research that the metal-poisoned catalyst has a silicon-rich surface, which indicates that silicon migrates in the catalyst particles. On the one hand, silicon reacts with aluminum on the catalyst surface to form amorphous aluminum silicate, causing blockage of the catalyst pores. On the other hand, silicon reacts with metal elements such as sodium, calcium, and iron brought by the crude oil to form dense components, which seriously reduce the activity of the catalyst. How to prevent the migration of silicon and improve the catalyst's ability to resist metal pollution has become the key to the research.
[0015] The inventors further discovered in their research that in the preparation method of the catalytic cracking catalyst provided by the present invention, by adopting a specific way to introduce a silicon source stabilizer and cooperate with the cracking active component, clay, and binder precursor, the melt sintering of the catalyst surface silicon and the contaminated metal in the prepared catalyst can be effectively slowed down, and the catalytic activity is significantly improved; then, by subjecting the microsphere particles to steam treatment at 100-500°C, the prepared catalytic cracking catalyst is further made to have excellent heavy oil conversion ability and resistance to metal pollution. The catalytic cracking catalyst is applied to heavy oil catalytic cracking, and has a high heavy oil conversion rate and a high total liquid product yield. The catalyst provided by the present invention has excellent resistance to multiple metal pollution, and in the case of iron, vanadium, and nickel pollution, it can have a higher total liquid product yield and a higher gasoline yield.
[0016] The second aspect of the present invention provides a catalytic cracking catalyst prepared by the preparation method described in the first aspect.
[0017] The third aspect of the present invention provides an application of the catalytic cracking catalyst described in the second aspect in the catalytic cracking of crude oil.
[0018] The beneficial effects of the present invention include:
[0019] The catalytic cracking catalyst prepared by the preparation method of the present invention has excellent heavy oil conversion ability, is applied to heavy oil catalytic cracking, and has a high heavy oil conversion rate and a high total liquid product yield. The catalyst provided by the present invention has excellent resistance to multiple metal pollution, and can have a higher total liquid product yield and a higher gasoline yield in the case of iron, vanadium and nickel pollution. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] One aspect of the present invention provides a method for preparing a catalytic cracking catalyst, the method comprising the following steps:
[0022] (1) performing a first mixing of a first binder precursor, a liquid medium, and a soluble compound of a silicon source stabilizer to obtain a first suspension, wherein the viscosity of the first suspension is not less than 10000 mPa·s;
[0023] (2) performing a second mixing of the first suspension with a cracking active component containing a Y molecular sieve, clay, and a second binder precursor to obtain a second suspension;
[0024] (3) spray drying the second suspension to obtain particle microspheres;
[0025] (4) treating the microspheres with steam at 100-500° C. to obtain a catalytic cracking catalyst;
[0026] Wherein, the soluble compound of the silicon source stabilizer is a soluble compound of a transition metal element;
[0027] The amount of the soluble compound of the silicon source stabilizer is such that in the prepared catalyst, the silicon source stabilizer accounts for 0.1-10% by weight of the dry basis of the catalyst, wherein the silicon source stabilizer is calculated as oxide.
[0028] In the present invention, the "soluble" means that the compound can be dissolved in a solvent directly or with the help of a co-solvent.
[0029] According to the present invention, preferably, the soluble compound of the silicon source stabilizer is at least one selected from the group consisting of soluble compounds of Group VIIB, Group VIII, Group IIB and Group IVB metals.
[0030] Preferably, the soluble compound of the silicon source stabilizer is selected from at least one of manganese-containing compounds, iron-containing compounds, cobalt-containing compounds, nickel-containing compounds, cadmium-containing compounds, zinc-containing compounds, titanium-containing compounds and zirconium-containing compounds, preferably selected from at least one of manganese-containing compounds, iron-containing compounds, zinc-containing compounds and zirconium-containing compounds.
[0031] Preferably, the silicon source stabilizer is selected from at least two of a manganese-containing compound, an iron-containing compound, a zinc-containing compound and a zirconium-containing compound.
[0032] More preferably, the soluble compound of the silicon source stabilizer is an iron-containing compound and a zinc-containing compound, and the amount of the iron-containing compound and the zinc-containing compound is such that the mass ratio of iron to zinc in the catalyst, calculated as oxide, is 0.1-1:1, preferably 0.1-0.5:1. By adopting this preferred embodiment, the migration activity of silicon under hydrothermal conditions can be effectively reduced, and the silicon enrichment on the catalyst surface can be slowed down.
[0033] According to the present invention, preferably, the manganese-containing compound is selected from at least one of manganese nitrate, manganese chloride and manganese sulfate; the iron-containing compound is selected from at least one of iron nitrate, iron chloride and iron sulfate; the zinc-containing compound is zinc chloride and / or zinc nitrate; the zirconium-containing compound is zirconium chloride and / or zirconium nitrate. The above substances are all conventionally selected in the art and can be obtained commercially.
[0034] According to the present invention, preferably, the amount of the soluble compound of the silicon source stabilizer is such that in the prepared catalyst, the silicon source stabilizer accounts for 0.1-2.5 weight% of the dry basis of the catalyst, for example, it can be 0.1 weight%, 0.2 weight%, 0.3 weight%, 0.4 weight%, 0.5 weight%, 0.6 weight%, 0.7 weight%, 0.8 weight%, 0.9 weight%, 1 weight%, 1.1 weight%, 1.2 weight%, 1.3 weight%, 1.4 weight%, 1.5 weight%, 1.6 weight%, 1.7 weight%, 1.8 weight%, 1.9 weight%, 2 weight%, 2.1 weight%, 2.2 weight%, 2.3 weight%, 2.4 weight%, 2.5 weight%, and any value in the range formed by any two of these values, wherein the silicon source stabilizer is calculated as oxide. By adopting this preferred embodiment, the migration activity of silicon under hydrothermal conditions can be further reduced, the silicon enrichment on the catalyst surface can be slowed down, and the hydrothermal stability of the catalyst can be improved. When the content of the silicon source stabilizer exceeds this range, the silicon source stabilizer will cover the acid center, resulting in a decrease in activity; when the content of the silicon source stabilizer is lower than this range, it is difficult to effectively capture active silicon.
[0035] According to the present invention, preferably, the amount of the cracking active component, clay and binder precursor is such that in the prepared catalyst, based on the total dry weight of the catalytic cracking catalyst, the content of the cracking active component is 1-60% by weight, preferably 10-50% by weight, for example, 1% by weight, 5% by weight, 10% by weight, 15% by weight, 20% by weight, 25% by weight, 30% by weight, 35% by weight, 40% by weight, 45% by weight, 50% by weight, 55% by weight, 60% by weight, and any value in the range formed by any two of these values; the content of clay is 1-70% by weight, preferably 5-65 ... 5 weight %, 30 weight %, 35 weight %, 40 weight %, 45 weight %, 50 weight %, 55 weight %, 60 weight %, 65 weight %, 70 weight %, and any value in the range formed by any two of these values; the content of the binder is 1-70 weight %, preferably 5-50 weight %, for example, it can be 1 weight %, 5 weight %, 10 weight %, 15 weight %, 20 weight %, 25 weight %, 30 weight %, 35 weight %, 40 weight %, 45 weight %, 50 weight %, 55 weight %, 60 weight %, 65 weight %, 70 weight %, and any value in the range formed by any two of these values; wherein the binder precursor is the sum of the first binder precursor and the second binder precursor. Adopting this preferred embodiment is conducive to improving the catalytic performance of the catalyst.
[0036] According to the present invention, preferably, the dry weight ratio of the first binder precursor to the second binder precursor is 1-5: 1, preferably 1-3: 1. This preferred embodiment is conducive to more uniformly dispersing the silicon source stabilizer inside the catalyst.
[0037] The present invention introduces the silicon source stabilizer by first mixing the first binder precursor, the liquid medium and the soluble compound of the silicon source stabilizer, which effectively ensures that the silicon source stabilizer has a higher contact efficiency with silicon and can also reduce the amount of the silicon source stabilizer.
[0038] The present invention has no particular limitation on the manner of adding the first binder precursor, the liquid medium and the soluble compound of the silicon source stabilizer in the first mixing process. They may be added together or separately, and the present invention does not impose any limitation on this.
[0039] In the prior art, the viscosity of the catalyst suspension is generally 2000-10000 mPa·s, while the viscosity of the first suspension is controlled at a higher level in the present invention, which is further conducive to encapsulating the silicon source stabilizer in the binder, thereby protecting the active center. Preferably, the viscosity of the first suspension is 10000-50000 mPa·s, preferably 12000-30000 mPa·s.
[0040] The present invention has no particular limitation on the method of controlling the viscosity of the first suspension, and conventional technical means in the art may be used. The present invention preferably uses the method of adjusting the amount of the liquid medium to achieve the purpose of regulating the viscosity of the first suspension.
[0041] Preferably, the solid content of the first suspension is 10-30 wt%.
[0042] The liquid medium of the present invention is a conventional choice in the art. Preferably, the liquid medium is an organic solvent and / or water, preferably water.
[0043] The present invention has no particular limitation on the amount of the liquid medium, provided that the viscosity of the first suspension is within the above range.
[0044] According to the present invention, preferably, the density of the first binder precursor is 1.1 g / cm 3 -1.5g / cm 3 , for example, can be 1.1 g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3and any value in the range formed by any two of these numerical values; the viscosity is 500-10000mPa·s, for example, it can be 500mPa·s, 1000mPa·s, 1500mPa·s, 2000mPa·s, 2500mPa·s, 3000mPa·s, 3500mPa·s, 4000mPa·s, 4500mPa·s, 5000mPa·s, 5500mPa·s, 6000mPa·s, 6500mPa·s, 7000mPa·s, 7500mPa·s, 8000mPa·s, 8500mPa·s, 9000mPa·s, 9500mPa·s, 10000mPa·s, and any value in the range formed by any two of these numerical values.
[0045] According to the present invention, preferably, the density of the second binder precursor is 1.3 g / cm 3 -1.6g / cm 3 , for example, can be 1.3 g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 and any value in the range formed by any two of these values; the viscosity is 500-5000mPa·s, for example, it can be 500mPa·s, 1000mPa·s, 1500mPa·s, 2000mPa·s, 2500mPa·s, 3000mPa·s, 3500mPa·s, 4000mPa·s, 4500mPa·s, 5000mPa·s, and any value in the range formed by any two of these values.
[0046] According to the present invention, preferably, the first binder precursor is a silicon-containing binder precursor, preferably silica sol and / or silica magnesium sol.
[0047] According to the present invention, preferably, the second binder precursor is an aluminum-containing binder precursor, preferably at least one selected from pseudo-boehmite, aluminum sol, phosphate aluminum sol and magnesium aluminum sol.
[0048] The inventors of the present invention have found during research that using a first binder precursor and a second binder precursor with specific characteristics (density, viscosity) and specific types is beneficial to improving the contact efficiency between the silicon source stabilizer and the active silicon.
[0049] The present invention has no particular limitation on the sources of the first binder precursor and the second binder precursor, as long as the above characteristic parameters are met.
[0050] The present invention has a wide range of selections for the type of the Y molecular sieve, which can be various Y molecular sieves commonly used in the art. The Y molecular sieve is an ion-modified Y molecular sieve and / or an ultra-stable Y molecular sieve.
[0051] Preferably, the ion modification includes at least one of rare earth ion modification, alkaline earth metal ion modification, transition metal ion modification and phosphorus modification.
[0052] Preferably, the Y-type molecular sieve is at least one selected from a Y-type molecular sieve containing rare earth, a Y-type molecular sieve containing phosphorus and rare earth, an ultrastable Y molecular sieve, and an ultrastable Y molecular sieve containing phosphorus and / or rare earth.
[0053] Further preferably, the Y-type molecular sieve is at least one selected from REHY molecular sieve, DOSY molecular sieve and DASY molecular sieve.
[0054] Preferably, the cracking active component further contains a second molecular sieve, and the second molecular sieve is selected from at least one of faujasite, Beta zeolite, MFI structure molecular sieve and mordenite. With this preferred embodiment, the product distribution can be flexibly adjusted, and in particular, the yield of light olefins can be improved.
[0055] The present invention has a wide range of choices for the types of faujasite, which can be a conventional choice in the art. Preferably, the faujasite is clinoptilolite and / or X-type zeolite.
[0056] The present invention has a wide range of selections for the types of the MFI structured molecular sieve, which can be a conventional choice in the art. Preferably, the MFI structured molecular sieve is a ZSM-5 molecular sieve.
[0057] Preferably, based on the total weight of the cracking active components, the content of the Y-type molecular sieve is 75% by weight or more, preferably 90% by weight or more, more preferably 95% by weight or more; the content of the second molecular sieve is 25% by weight or less, preferably 10% by weight or less, more preferably 5% by weight or less.
[0058] The present invention has a wide range of clay types, and can be any existing clay that can be used in catalytic cracking catalysts. Preferably, the clay is selected from at least one of kaolin, montmorillonite, diatomaceous earth, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite.
[0059] The present invention has no particular limitation on the order of adding the first suspension, the cracking active component containing Y molecular sieve, clay, and the second binder precursor in the second mixing process, and they can be added together or separately. The present invention preferably adopts the method of adding the first suspension, clay, the cracking active component containing Y molecular sieve, and the second binder precursor in sequence.
[0060] According to a preferred embodiment of the present invention, the cracking active component is provided in the form of a first slurry, and the liquid medium in the first slurry is the same as the liquid medium in step (1).
[0061] The present invention has no particular limitation on the amount of the liquid medium in the first slurry, and it can be selected conventionally in the art.
[0062] According to a preferred embodiment of the present invention, the clay is provided in the form of a second slurry, and the liquid medium in the second slurry is the same as the liquid medium in the first slurry.
[0063] The present invention has no particular limitation on the amount of the liquid medium in the second slurry, and it can be selected conventionally in the art.
[0064] Preferably, the second mixing is performed under stirring conditions.
[0065] The present invention has no particular limitation on the stirring rate and time, which can be appropriately selected according to the specific situation, as long as the purpose of uniform mixing can be achieved.
[0066] The present invention has no particular limitation on the specific conditions of the spray drying in step (3), and the spray drying can be carried out according to conventional methods in the art, as long as the requirements for catalyst particle size and strength in the catalytic cracking of crude oil are met.
[0067] The steam treatment of the present invention is beneficial to further improve the heavy oil conversion ability and metal pollution resistance of the catalyst. Preferably, the conditions of the steam treatment in step (4) include: a temperature of 250-350°C, for example, it can be 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, and any value in the range formed by any two of these values; the time is 2-8h. The use of this preferred embodiment is conducive to the efficient combination of active silicon and silicon source stabilizer. When the temperature of the steam treatment exceeds this range, the active center will be damaged; when the temperature of the steam treatment is lower than this range, the active silicon cannot be effectively combined with the silicon source stabilizer.
[0068] Preferably, the volume space velocity of the water vapor is 0.2-1h -1 , preferably 0.2-0.8h -1 The use of this preferred embodiment is further conducive to efficiently combining active silicon with the silicon source stabilizer.
[0069] According to a particularly preferred embodiment of the present invention, a method for preparing a catalytic cracking catalyst comprises the following steps:
[0070] (1) performing a first mixing of a first binder precursor, a liquid medium and a soluble compound of a silicon source stabilizer to obtain a first suspension, wherein the viscosity of the first suspension is 12000-30000 mPa·s;
[0071] (2) performing a second mixing of the first suspension with a cracking active component containing a Y molecular sieve, clay, and a second binder precursor to obtain a second suspension;
[0072] (3) spray drying the second suspension to obtain particle microspheres;
[0073] (4) treating the microspheres with steam at 250-350° C. to obtain a catalytic cracking catalyst;
[0074] The volume space velocity of the water vapor is 0.2-0.8h -1 ;
[0075] The soluble compounds of the silicon source stabilizer are iron-containing compounds and zinc-containing compounds, and the amounts of the iron-containing compounds and the zinc-containing compounds are such that the mass ratio of iron to zinc in the catalyst, calculated as oxides, is 0.1-0.5:1;
[0076] The amount of the soluble compound of the silicon source stabilizer is such that in the prepared catalyst, the silicon source stabilizer accounts for 0.1-2.5% by weight of the dry basis of the catalyst, wherein the silicon source stabilizer is calculated as oxide.
[0077] The catalytic cracking catalyst prepared by the preparation method of the present invention has excellent heavy oil conversion ability, is applied to heavy oil catalytic cracking, and has a high heavy oil conversion rate and a high total liquid product yield. The catalyst prepared by the preparation method of the present invention has excellent resistance to multiple metal pollution, and can have a higher total liquid product yield and a higher gasoline yield in the case of iron, vanadium, and nickel pollution.
[0078] In the present invention, the "first" and "second" do not limit the substances and operations, but are only used to distinguish the substances introduced in different steps and the operations performed in different stages.
[0079] A second aspect of the present invention provides a catalytic cracking catalyst as described in the first aspect.
[0080] According to the present invention, preferably, based on the total dry weight of the catalytic cracking catalyst, the content of the silicon source stabilizer is 0.1-10% by weight, preferably 0.1-2.5% by weight; the content of the cracking active component is 1-60% by weight, preferably 10-50% by weight; the content of the clay is 1-70% by weight, preferably 5-65% by weight; the content of the binder is 1-70% by weight, preferably 5-50% by weight, wherein the binder is the sum of the first binder and the second binder.
[0081] According to the present invention, preferably, the dry mass ratio of the first binder to the second binder is 1-5:1, preferably 1-3:1.
[0082] The third aspect of the present invention provides an application of the catalytic cracking catalyst described in the second aspect in the catalytic cracking of crude oil.
[0083] In order to better illustrate the anti-metal pollution performance of the catalyst described in the present invention, the test example of the present invention uses a catalyst impregnated with 3000ppm iron, 3000ppm nickel, and 3000ppm vanadium to simulate the catalyst in which the polluted metal elements reach equilibrium after long-term operation in actual applications.
[0084] The present invention has no particular limitation on the method for metal contamination, and the conventional method of the present invention can be used. The present invention uses the Mitchell method as an example (Mitchell BR. Metal Contamination of Cracking Catalysts. 1. Synthetic Metals Deposition on Fresh Catalysts [J]. Industrial & Engineering Chemistry Product Research and Development, 1980, 19 (2): 209-213).
[0085] In order to detect the stability of the catalyst, the metal-contaminated catalyst is subjected to an aging treatment before use. The present invention has no particular limitation on the conditions of the aging treatment, and the aging treatment can be carried out using conventional methods in the art.
[0086] The present invention will be described in detail below through examples.
[0087] DASY molecular sieve (solid content of 92 weight percent, RE2O3 of 1.8 weight percent, Na2O of 1 weight percent, and crystallinity of 60%), Beta molecular sieve (solid content of 95.2 weight percent, Na2O of 1.2 weight percent, and crystallinity of 60%), and ZSM-5 molecular sieve (solid content of 95 weight percent, and crystallinity of 85%) are all produced by Sinopec Catalyst Qilu Branch.
[0088] In the following examples, all raw materials involved are commercially available unless otherwise specified.
[0089] Example 1
[0090] This example is used to illustrate the catalytic cracking catalyst and its preparation method provided by the present invention.
[0091] The density is 1.1 g / cm 3 , the first binder silica sol with a viscosity of 5000 mPa·s and ferric chloride were mixed, and then water was added to make the viscosity of the first suspension 20000 mPa·s and the solid content 15 wt%. The slurry containing kaolin (solid content 25 wt%) was added to the first suspension, stirred for 30 min, and then the slurry containing molecular sieves DASY and ZSM-5 (solid content 25 wt%) was added, and the stirring was continued for 20 min. Finally, a slurry with a density of 1.3 g / cm 3 , and a second binder aluminum sol with a viscosity of 500 mPa·s to obtain a second suspension. The second suspension is spray-dried at 450°C to obtain particle microspheres. The particle microspheres are treated with water vapor at 250°C, and the space velocity of the water vapor is 0.5 h -1 , catalytic cracking catalyst C1 was obtained, and the composition characteristics of the catalyst are listed in Table 1.
[0092] Example 2
[0093] The density is 1.3 g / cm 3 , the first binder silica sol with a viscosity of 8000 mPa·s and zinc chloride were mixed, and then water was added to make the viscosity of the first suspension 15000 mPa·s and the solid content 15 wt%. The slurry containing kaolin (solid content 25 wt%) was added to the first suspension and stirred for 30 min, and then the slurry containing molecular sieves DASY, β (solid content 25 wt%) was added and stirred for 20 min, and finally the slurry with a density of 1.4 g / cm 3 , and a second binder phosphoaluminum sol with a viscosity of 1000 mPa·s to obtain a second suspension. The second suspension is spray-dried at 450°C to obtain particle microspheres. The particle microspheres are treated with water vapor at 300°C, and the space velocity of the water vapor is 0.3 h -1 , catalytic cracking catalyst C2 was obtained, and the composition characteristics of the catalyst are listed in Table 1.
[0094] Example 3
[0095] The density is 1.1 g / cm 3, the first binder silica sol with a viscosity of 2000 mPa·s and zirconium chloride were mixed, and then water was added to make the viscosity of the first suspension 18000 mPa·s and the solid content 15 wt %. The slurry containing kaolin (solid content 25 wt %) was added to the first suspension, stirred for 30 min, and then the slurry containing molecular sieve DASY (solid content 25 wt %) was added, and stirred for 20 min, and finally the slurry with a density of 1.3 g / cm 3 , and a second binder magnesium aluminum sol with a viscosity of 3000mPa·s to obtain a second suspension. The second suspension is spray-dried at 450°C to obtain particle microspheres. The particle microspheres are treated with water vapor at 320°C, and the space velocity of the water vapor is 0.5h -1 , catalytic cracking catalyst C3 was obtained, and the composition characteristics of the catalyst are listed in Table 1.
[0096] Example 4
[0097] The density is 1.1 g / cm 3 , the first binder silica sol with a viscosity of 2000 mPa·s was mixed with ferric chloride and zinc chloride, and then water was added to make the viscosity of the first suspension 13000 mPa·s and the solid content 15 wt%. The slurry containing kaolin (solid content 25 wt%) was added to the first suspension and stirred for 30 min, and then the slurry containing molecular sieves DASY and ZSM-5 (solid content 25 wt%) was added and stirred for 20 min, and finally the slurry with a density of 1.3 g / cm 3 , and a second binder aluminum sol with a viscosity of 500 mPa·s to obtain a second suspension. The second suspension is spray-dried at 450°C to obtain particle microspheres. The particle microspheres are treated with water vapor at 250°C, and the space velocity of the water vapor is 0.5 h -1 , catalytic cracking catalyst C4 was obtained, and the composition characteristics of the catalyst are listed in Table 1.
[0098] Example 5
[0099] The method of Example 1 is followed, except that the amount of silicon source stabilizer added is such that in the prepared catalyst, the silicon source stabilizer accounts for 3 weight % of the dry basis of the catalyst, wherein the silicon source stabilizer is calculated as oxide, to obtain catalytic cracking catalyst C5, the composition characteristics of the catalyst are listed in Table 1.
[0100] Example 6
[0101] The method of Example 1 was followed, except that the particle microspheres were treated with steam at 100° C. to obtain catalytic cracking catalyst C6. The composition characteristics of the catalyst are listed in Table 1.
[0102] Example 7
[0103] The method of Example 1 is followed, except that the particle microspheres are treated with steam at 500° C. to obtain catalytic cracking catalyst C7. The composition characteristics of the catalyst are listed in Table 1.
[0104] Comparative Example 1
[0105] The method of Example 1 was followed, except that no silicon source stabilizer was added, to obtain catalytic cracking catalyst D1. The composition characteristics of the catalyst are listed in Table 1.
[0106] Comparative Example 2
[0107] The method of Example 1 was followed, except that the microsphere particles were not treated with steam but were directly calcined at 500° C. for 1 hour to obtain catalytic cracking catalyst D2. The composition characteristics of the catalyst are listed in Table 1.
[0108] Table 1
[0109]
[0110] Test Example 1
[0111] The catalytic cracking catalysts prepared in the above examples and comparative examples were impregnated with 3000ppm of contaminated iron, 3000ppm of nickel and 3000ppm of vanadium respectively by the Mitchell method, that is, vanadium cyclopentaneate was used as the vanadium source, nickel cyclopentaneate was used as the nickel source, iron cyclopentaneate was used as the iron source, and toluene was used as the solvent to prepare a metal-containing solution. The catalyst was impregnated in the metal-containing solution, then dried, and then calcined at about 600°C to remove organic matter. Aging treatment was performed at 780°C and 100% water vapor for 4 hours, and the cracking performance was evaluated on a small fixed fluidized bed. The evaluation conditions of the heavy oil micro-reactor are: the weight ratio of catalyst to raw oil (catalyst-to-oil ratio) is 5, the catalyst loading is 9g, the reaction temperature is 520°C, and the WHSV is 8h -1 , oil inlet time 70 seconds, the feed oil is vacuum gas oil. The properties of the feed oil are shown in Table 2. The evaluation results are listed in Table 3.
[0112] Table 2
[0113]
[0114] Table 3
[0115]
[0116] Note: Conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield;
[0117] Total liquid product yield = gasoline yield + diesel yield + liquefied gas yield.
[0118] It can be seen from the results in Table 3 that the catalytic cracking catalyst prepared by the preparation method of the present invention has excellent heavy oil conversion ability, and is applied to heavy oil catalytic cracking, and has a high heavy oil conversion rate and a high total liquid product yield. The catalyst provided by the present invention has excellent resistance to multiple metal pollution, and can have a higher total liquid product yield and a higher gasoline yield in the case of iron, vanadium, and nickel pollution.
[0119] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a catalytic cracking catalyst, the method comprising the following steps: (1) A first binder precursor, a liquid medium and a soluble compound of a silicon source stabilizer are first mixed to obtain a first suspension, wherein: The viscosity of the first suspension is not less than 10000 mPa·s; (2) performing a second mixing of the first suspension with a cracking active component containing a Y molecular sieve, clay, and a second binder precursor to obtain a second suspension; (3) spray drying the second suspension to obtain particle microspheres; (4) treating the microspheres with steam at 100-500° C. to obtain a catalytic cracking catalyst; Wherein, the soluble compound of the silicon source stabilizer is a soluble compound of a transition metal element; The amount of the soluble compound of the silicon source stabilizer is such that in the prepared catalyst, the silicon source stabilizer accounts for 0.1-10% by weight of the dry basis of the catalyst, wherein the silicon source stabilizer is calculated as oxide.
2. The preparation method according to claim 1, wherein The soluble compound of the silicon source stabilizer is selected from at least one of soluble compounds of Group VIIB, Group VIII, Group IIB and Group IVB metals; Preferably, the soluble compound of the silicon source stabilizer is selected from at least one of a manganese-containing compound, an iron-containing compound, a zinc-containing compound and a zirconium-containing compound; More preferably, the soluble compound of the silicon source stabilizer is an iron-containing compound and a zinc-containing compound, and the amount of the iron-containing compound and the zinc-containing compound is such that the mass ratio of iron to zinc in the catalyst, calculated as oxide, is 0.1-1:1, preferably 0.1-0.5:1; Preferably, the manganese-containing compound is selected from at least one of manganese nitrate, manganese chloride and manganese sulfate; the iron-containing compound is selected from at least one of iron nitrate, iron chloride and iron sulfate; the zinc-containing compound is zinc chloride and / or zinc nitrate; and the zirconium-containing compound is zirconium chloride and / or zirconium nitrate.
3. The preparation method according to claim 1, wherein The soluble compound of the silicon source stabilizer is used in an amount such that in the prepared catalyst, the silicon source stabilizer accounts for 0.1-2.5% by weight of the dry basis of the catalyst, wherein the silicon source stabilizer is calculated as oxide; Preferably, the amounts of the cracking active component, clay and binder precursor are such that in the prepared catalyst, based on the total dry weight of the catalytic cracking catalyst, the content of the cracking active component is 1-60% by weight, preferably 10-50% by weight; the content of the clay is 1-70% by weight, preferably 5-65% by weight; the content of the binder is 1-70% by weight, preferably 5-50% by weight, wherein the binder precursor is the sum of the first binder precursor and the second binder precursor; Preferably, the dry weight ratio of the first binder precursor to the second binder precursor is 1-5:1, preferably 1-3:
1.
4. The preparation method according to any one of claims 1 to 3, wherein The said 一 The viscosity of the suspension is 10000-50000 mPa·s, preferably 12000-30000 mPa·s; Preferably, the liquid medium is an organic solvent and / or water, preferably water.
5. The preparation method according to any one of claims 1 to 4, wherein: The density of the first binder precursor is 1.1 g / cm 3 -1.5g / cm 3 , viscosity is 500-10000mPa·s; Preferably, the density of the second binder precursor is 1.3 g / cm 3 -1.6g / cm 3 , viscosity is 500-5000mPa·s; Preferably, the first binder precursor is a silicon-containing binder precursor, preferably silica sol and / or silica-magnesium sol; The second binder precursor is an aluminum-containing binder precursor, and is preferably selected from at least one of pseudo-boehmite, aluminum sol, phosphate aluminum sol and magnesium aluminum sol.
6. The preparation method according to any one of claims 1 to 5, wherein: The Y molecular sieve is an ion-modified Y molecular sieve and / or an ultra-stable Y molecular sieve; Preferably, the ion modification includes at least one of rare earth ion modification, alkaline earth metal ion modification, transition metal ion modification and phosphorus modification; Preferably, the Y-type molecular sieve is at least one selected from a Y-type molecular sieve containing rare earth, a Y-type molecular sieve containing phosphorus and rare earth, an ultra-stable Y molecular sieve, and an ultra-stable Y molecular sieve containing phosphorus and / or rare earth; Further preferably, the Y-type molecular sieve is at least one selected from REHY molecular sieve, DOSY molecular sieve and DASY molecular sieve; Preferably, the cracking active component further contains a second molecular sieve, and the second molecular sieve is selected from at least one of faujasite, Beta zeolite, MFI structure molecular sieve and mordenite; Preferably, based on the total weight of the cracking active components, the content of the Y-type molecular sieve is 75% by weight or more, preferably 90% by weight or more, more preferably 95% by weight or more; the content of the second molecular sieve is 25% by weight or less, preferably 10% by weight or less, more preferably 5% by weight or less.
7. The preparation method according to any one of claims 1 to 6, wherein: The clay is selected from at least one of kaolin, montmorillonite, diatomaceous earth, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite.
8. The preparation method according to any one of claims 1 to 7, wherein: The conditions of the water vapor treatment in step (4) include: a temperature of 250-350° C. and a time of 2-8 h; Preferably, the volume space velocity of the water vapor is 0.2-1h -1 , preferably 0.2-0.8h -1 .
9. A catalytic cracking catalyst prepared by the preparation method according to any one of claims 1 to 8; Preferably, based on the total dry weight of the catalytic cracking catalyst, the content of the silicon source stabilizer is 0.1-10% by weight, preferably 0.1-2.5% by weight; the content of the cracking active component is 1-60% by weight, preferably 10-50% by weight; the content of the clay is 1-70% by weight, preferably 5-65% by weight; the content of the binder is 1-70% by weight, preferably 5-50% by weight, wherein, The binder is the sum of the first binder and the second binder; Preferably, the dry basis mass ratio of the first binder to the second binder is 1-5:1, preferably 1-3:
1.
10. Use of the catalytic cracking catalyst according to claim 9 in catalytic cracking of crude oil.