Beneficiation and recovery method for calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ore

Through preferential mixed flotation of molybdenum bismuth and chemical combination capture measures, the interference of calcium and magnesium gangue on molybdenum bismuth sulfur ore is solved, and efficient recovery of molybdenum bismuth sulfur polymetallic ore is achieved, improving ore dressing indicators and recovery rates are reduced. Cost and mine circulation.

CN119056578AActive Publication Date: 2024-12-03CHINA MINMETALS CHANGSHA MINING RES INST
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411327557.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

The existing ore dressing technology is prone to mudification when treating calcium-magnesium gangue-containing molybdenum bismuth sulfur polymetallic ore, which leads to the ore slurry becoming sticky and suspended and not easily settled, affecting the molybdenum bismuth sulfur flotation effect, and the existing methods require strong force. Collectants or highly selective agents lead to high costs and low metal recovery.

Method used

The process of preferential mixing of molybdenum bismuth partial flotation-residual bismuth and sulfur flotation-molybdenum bismuth separation-bismuth sulfur separation, and the combination of chemical B11+F9 capture and mineral sludge inhibitor CD-N1 are adopted to reduce calcium and magnesium sludge The interference of ganglite enhances the ore dressing process in stages.

Benefits of technology

The ore dressing recovery efficiency and indicators of molybdenum, bismuth and sulfur are improved, and the problems of difficulty in separation of molybdenum, bismuth and sulfur are avoided. The problem of low metal recovery is achieved. The efficient recovery of molybdenum, bismuth and sulfur is reduced, and the cost of drug use and ore circulation is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056578A_ABST
    Figure CN119056578A_ABST
Patent Text Reader

Abstract

The invention provides a beneficiation and recovery method for calcium-magnesium-containing gangue type molybdenum-bismuth-sulfur polymetallic ore, which comprises the following steps: firstly recovering molybdenum and part of bismuth with good floatability, then recovering the rest of bismuth and sulfur with poor floatability, and finally respectively obtaining the final molybdenum concentrate, the final bismuth concentrate and the final sulfur concentrate through molybdenum-bismuth separation and bismuth-sulfur separation. The beneficiation process scheme of molybdenum and bismuth part preferential bulk flotation, residual bismuth and sulfur flotation, molybdenum and bismuth separation and bismuth and sulfur separation is adopted, and measures such as combined collection of reagents B11 and F9, bubbling recovery of molybdenum and part of bismuth with good floatability, inhibition of calcium and magnesium argillaceous gangue minerals by CD-N1 and the like are taken. Interference of calcium-magnesium argillaceous gangue on the enrichment and separation process of molybdenum, bismuth and sulfur is reduced, the beneficiation process is strengthened in stages, and the beneficiation recovery efficiency and indexes of molybdenum, bismuth and sulfur are improved. The method effectively solves the problem of efficient recovery of calcium-magnesium-containing gangue type molybdenum-bismuth-sulfur polymetallic ore, the process is simple and reliable, the reagent system is efficient, and a new effective method is provided for recovery of similar molybdenum-bismuth-sulfur resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore dressing, and in particular to a ore dressing and recovery method for a calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ore. Background Art

[0002] The calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore is a molybdenum-bismuth-sulfur resource that contains a certain amount of calcium-magnesium carbonate or silicate minerals such as calcite, dolomite, grossular garnet, tremolite, actinolite, and diopside. The existing mineral processing and recovery technology is mainly flotation. When it is applied to this type of ore, the calcium-magnesium gangue is easy to become mud after grinding, and it continuously dissolves and releases Ca in the slurry. 2+ Mg 2+ These metal cations will consume the molybdenum-bismuth flotation reagents on the one hand, and on the other hand, they will cover the surface of the molybdenum-bismuth minerals through electrostatic action and affect the flotation effect. At the same time, they will have a dispersing effect on the pulp, causing the pulp to become sticky, suspended and difficult to settle, and a large amount of intermediate ore circulation, which will have a great impact on the molybdenum-bismuth-sulfur flotation process and result in poor molybdenum-bismuth-sulfur beneficiation indicators.

[0003] At present, the flotation processes for this type of molybdenum, bismuth and sulfur resources mainly include two methods: "molybdenum, bismuth and sulfur mixed flotation-molybdenum, bismuth and sulfur separation" and "molybdenum, bismuth and other floatable-molybdenum, bismuth separation-tailing flotation sulfur". For example, the invention patent (application number CN 202310854562.1) discloses a flotation and efficient recovery method for low-grade molybdenum, bismuth and sulfur polymetallic ores. First, the raw ore is ground and classified to form a pulp, and flotation agents are added to carry out full flotation roughing of sulfide ore, flotation concentration, full flotation scavenging, flotation scavenging, grinding, and full flotation concentration re-selection. The full flotation concentrate can be separated to obtain molybdenum concentrate, bismuth concentrate, copper concentrate and sulfur concentrate products. The invention patent (application number CN 202111460430.8) discloses an efficient and non-toxic molybdenum, bismuth and sulfur recovery method, step one: sulfide ore fully floated mixed concentrate for molybdenum, bismuth and sulfur separation, step two: add lime, kerosene, sulfur inhibitor, and water glass to the ore sample in step one in turn for molybdenum, bismuth and sulfur separation to obtain a molybdenum, bismuth and mixed concentrate, and the tailings are sulfur concentrates, step three: the molybdenum, bismuth and mixed concentrate obtained in step two is subjected to molybdenum, bismuth and mixed separation, the scraped foam is the molybdenum concentrate, and the tailings are the bismuth concentrate. However, in the two methods of "molybdenum, bismuth and sulfur mixed flotation-molybdenum, bismuth and sulfur separation" and "molybdenum, bismuth and other floatable-molybdenum, bismuth and sulfur separation-tailings flotation sulfur", the former requires the addition of a strong collector, calcium and magnesium gangue are easily entrained and floated, and the separation of molybdenum, bismuth and sulfur is difficult and costly, while the latter requires the use of a highly selective collector, and the metal recovery rate is relatively low.

[0004] In recent years, some researchers have adopted the scheme of "coarse grinding of raw ore-centralized re-grinding of intermediate ore-step-enhanced separation of molybdenum, bismuth and sulfur" to strengthen the recovery of difficult-to-float molybdenum, bismuth and sulfur minerals. For example, the invention patent (application number CN 202211174476.8) discloses a beneficiation method for efficient recovery of low-grade molybdenum, bismuth and sulfur polymetallic ores by step-enhanced flotation. However, this scheme does not have corresponding measures for calcium-magnesium gangue, so it is not completely suitable for the recovery of molybdenum, bismuth and sulfur resources containing calcium-magnesium gangue.

[0005] In view of this, it is necessary to design an improved mineral processing and recovery method for calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ore to solve the above problems. Summary of the invention

[0006] The object of the present invention is to provide a beneficiation and recovery method for a calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ore, which adopts a beneficiation process of partial preferential mixed flotation of molybdenum and bismuth-remaining bismuth and sulfur flotation-molybdenum-bismuth separation-bismuth-sulfur separation, and adopts measures such as combined capture-foaming recovery of molybdenum and part of bismuth by reagent B11+F9, and inhibition of calcium-magnesium muddy gangue minerals by CD-N1, so as to reduce the interference of calcium-magnesium muddy gangue on the enrichment and separation process of molybdenum, bismuth and sulfur, strengthen the beneficiation process in stages, and improve the beneficiation and recovery efficiency and indicators of molybdenum, bismuth and sulfur.

[0007] To achieve the above-mentioned purpose of the invention, the present invention provides a method for beneficiation and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore, comprising the following steps:

[0008] S1. Crushing and grinding the raw ore to obtain a grinding product in which the ore powder with a fineness of less than 0.074 mm accounts for 78% to 83% of the total mass, and adding water to the grinding product to a pulp concentration of 30% to 35%;

[0009] S2, adding molybdenum-bismuth collector B11 and frother F9 to the slurry obtained in step S1, and performing partial preferential mixed flotation of molybdenum-bismuth to obtain molybdenum-bismuth mixed coarse concentrate and molybdenum-bismuth flotation tailings;

[0010] S3, subjecting the molybdenum-bismuth mixed coarse concentrate of step S2 to two closed-circuit pre-concentrations to obtain a molybdenum-bismuth mixed concentrate, wherein the slime inhibitor CD-N1 is added in both closed-circuit pre-concentration steps; subjecting the molybdenum-bismuth mixed concentrate to molybdenum-bismuth separation flotation to obtain a molybdenum concentrate and a first bismuth concentrate;

[0011] S4, adding a slime inhibitor CD-N1, an activator, a collector and a frother F9 to the molybdenum-bismuth flotation tailings of step S2 in sequence to carry out flotation roughing of the remaining bismuth and sulfur to obtain a bismuth-sulfur rough concentrate and a bismuth-sulfur flotation tailings;

[0012] S5, subjecting the bismuth-sulfur coarse concentrate of step S4 to two closed-circuit pre-concentrations to obtain a bismuth-sulfur mixed concentrate, wherein the slime inhibitor CD-N1 is added in both closed-circuit pre-concentration steps; subjecting the bismuth-sulfur mixed concentrate to bismuth-sulfur separation flotation to obtain a second bismuth concentrate and a sulfur concentrate;

[0013] S6. The bismuth-sulfur flotation tailings of step S4 are subjected to three closed-circuit scavenging processes to obtain final tailings, and the intermediate ores obtained in the three scavenging processes are returned to the previous process step by step.

[0014] As a further improvement of the present invention, the components of the molybdenum-bismuth collector B11 include, by mass percentage, 40% to 50% of mineral oil, 30% to 40% of diesel, 10% to 20% of O-isopropyl-N-ethylthiocarbamate and 10% to 20% of polyoxypropylene ether; the foaming agent F9 includes, by mass percentage, 50% to 70% of triethoxybutyl ether, 20% to 30% of methyl isobutyl carbinol and 20% to 40% of camphor oil; the slime inhibitor CD-N1 includes, by mass percentage, 40% to 50% of hydroxyethyl cellulose, 10% to 30% of locust bean gum and 20% to 30% of lactic acid.

[0015] As a further improvement of the present invention, in step S2, the added amount of the molybdenum-bismuth collector B11 is 80-120 g / t, and the added amount of the foaming agent F9 is 20-40 g / t.

[0016] As a further improvement of the present invention, in step S3, the middlings produced by the first closed-circuit pre-concentration are returned to the molybdenum-bismuth part of step S2 for preferential mixed flotation, and the middlings produced by the second closed-circuit pre-concentration are returned to the first closed-circuit pre-concentration. The amount of the slime inhibitor CD-N1 added in the first closed-circuit pre-concentration is 40-60 g / t, and the amount of the slime inhibitor CD-N1 added in the second closed-circuit pre-concentration is 10-30 g / t; activated carbon is added for scrubbing and drug removal during the molybdenum-bismuth separation flotation, and sodium sulfide or sodium hydrosulfide is selected as the bismuth inhibitor.

[0017] As a further improvement of the present invention, in step S4, the added amount of the slime inhibitor CD-N1 is 180-220 g / t, the activator is copper sulfate, and the added amount is 130-170 g / t, the collectors are butyl xanthate and ethyl thiocyanate, and the added amounts are 80-120 g / t and 10-30 g / t respectively, and the added amount of the foaming agent F9 is 10-20 g / t.

[0018] As a further improvement of the present invention, in step S5, the middlings produced by the first closed-circuit pre-concentration are returned to the flotation roughing of the remaining bismuth and sulfur in step S4, and the middlings produced by the second closed-circuit pre-concentration are returned to the first closed-circuit pre-concentration. The amount of the slime inhibitor CD-N1 added in the first closed-circuit pre-concentration is 80-120 g / t, and the amount of the slime inhibitor CD-N1 added in the second closed-circuit pre-concentration is 40-60 g / t; activated carbon is added for scrubbing and removing the drug during the bismuth-sulfur separation flotation, and lime and sodium humate are selected as the sulfur inhibitor.

[0019] As a further improvement of the present invention, in step S6, 50-100 g / t of slime inhibitor CD-N1, 30-50 g / t of butyl xanthate and 2-7 g / t of frother F9 are added to the three closed-circuit sweeps, the intermediate ore from the first closed-circuit sweep is returned to the rough flotation of the remaining bismuth and sulfur in step S4, and the intermediate ore from the second and third closed-circuit sweeps is returned to the previous sweep in turn.

[0020] As a further improvement of the present invention, the process of molybdenum-bismuth separation flotation is a combination of one coarse three, four, five, six fine two, three, four scavenging, the amount of activated carbon used is 100-500g / t, the amount of sodium sulfide used is 200-8000g / t, or the amount of sodium hydrosulfide used is 100-6000g / t.

[0021] As a further improvement of the present invention, the bismuth-sulfur separation flotation process is a combination of one coarse two, three, four, five fine two, three, four scavenging, the amount of activated carbon is 100-500g / t, the amount of lime is 500-10000g / t, and the amount of sodium humate is 20-300g / t.

[0022] As a further improvement of the present invention, in step S1, the grade of the ore is: Mo grade 0.05%-0.15%, Bi grade 0.05%-0.2%, S grade 0.5%-4.5%; the calcite content is 2%-8%, the dolomite content is 0.5%-5%, the grossular garnet content is 10%-25%, the tremolite content is 1%-10%, the actinolite content is 1%-10%, and the diopside content is 1%-10%.

[0023] The beneficial effects of the present invention are:

[0024] 1. The present invention provides a method for the beneficiation and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore. Based on the commonality of the floatability of molybdenum, bismuth and sulfur minerals, the beneficiation process is rationally designed to preferentially recover molybdenum and part of the bismuth with good floatability, and then recover the remaining bismuth and sulfur with poor floatability. Finally, the final molybdenum, bismuth and sulfur concentrates are obtained by molybdenum-bismuth separation and bismuth-sulfur separation. The new beneficiation process scheme of the present invention effectively solves the interference of the large difference in floatability of bismuth minerals on the recovery and separation of molybdenum-bismuth-sulfur, and maximizes the avoidance of the problems of difficulty in separating molybdenum-bismuth-sulfur and poor indicators under the "molybdenum-bismuth-sulfur mixed floatation-molybdenum-bismuth-sulfur separation" process in the prior art and the low metal recovery rate under the "molybdenum-bismuth-sulfur mixed floatation-molybdenum-bismuth-sulfur separation-tailings floating sulfur" process. By strengthening the beneficiation process in stages, the beneficiation recovery efficiency and indicators of molybdenum, bismuth and sulfur are improved, and the problem of efficient recovery and utilization of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore is solved.

[0025] 2. The present invention adopts a beneficiation process of partial preferential mixed flotation of molybdenum and bismuth - flotation of remaining bismuth and sulfur - separation of molybdenum and bismuth - separation of bismuth and sulfur, and recovers molybdenum and part of bismuth with good floatability through combined capture and bubbling of reagents B11+F9. Through the reasonable selectivity of the collector system, the entrainment and flotation of calcium-magnesium muddy gangue is effectively avoided, and the rapid and efficient recovery of molybdenum and bismuth is achieved, while providing good molybdenum-bismuth mixed concentrate conditions for molybdenum-bismuth separation and flotation. At the same time, on the basis of using a strong collector, the reagent CD-N1 is used as an efficient calcium-magnesium gangue inhibitor, which effectively reduces the interference of calcium-magnesium muddy gangue on the flotation and concentration process of bismuth-sulfur minerals, and provides conditions for the full and efficient recovery of bismuth and sulfur.

[0026] 3. The present invention uses a reasonable segmented recovery process of molybdenum, bismuth and sulfur, and cooperates with independently developed reagents to efficiently capture metal ores and effectively regulate calcium-magnesium mudstone, so that the cost of reagent use is low, the difficulty of separating molybdenum, bismuth and bismuth sulfur is small, the amount of ore circulation in the main process is small, and the process flow is highly stable. This method effectively solves the problem of efficient recovery of calcium-magnesium gangue-containing molybdenum, bismuth and sulfur polymetallic ores, has a simple and reliable process, and an efficient reagent system, providing a new and effective method for the recovery of similar molybdenum, bismuth and sulfur resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is a schematic flow chart of the mineral processing and recovery method of the calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ore. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0029] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0030] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0031] See also Figure 1 As shown, a method for beneficiation and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore comprises the following steps:

[0032] S1. Crushing and grinding the raw ore to obtain a grinding product in which the ore powder with a fineness of less than 0.074 mm accounts for 78% to 83% of the total mass, and adding water to the grinding product to a slurry concentration of 30% to 35%; wherein the grade of the raw ore is: Mo grade 0.05% to 0.15%, Bi grade 0.05% to 0.2%, S grade 0.5% to 4.5%; the content of calcite is 2% to 8%, the content of dolomite is 0.5% to 5%, the content of grossular garnet is 10% to 25%, the content of tremolite is 1% to 10%, the content of actinolite is 1% to 10%, and the content of diopside is 1% to 10%;

[0033] S2. Adding molybdenum-bismuth collector B11 and frother F9 to the ore pulp obtained in step S1, and performing partial preferential mixed flotation of molybdenum-bismuth to obtain molybdenum-bismuth mixed coarse concentrate and molybdenum-bismuth flotation tailings; wherein the addition amount of molybdenum-bismuth collector B11 is 80-120 g / t, and the addition amount of frother F9 is 20-40 g / t;

[0034] S3, subjecting the molybdenum-bismuth mixed coarse concentrate of step S2 to two closed-circuit pre-concentrations to obtain a molybdenum-bismuth mixed concentrate, wherein the slime inhibitor CD-N1 is added in both closed-circuit pre-concentration steps; subjecting the molybdenum-bismuth mixed concentrate to molybdenum-bismuth separation flotation to obtain a molybdenum concentrate and a first bismuth concentrate;

[0035] S4, the molybdenum-bismuth flotation tailings of step S2 are sequentially added with a slime inhibitor CD-N1, an activator, a collector and a frother F9 to carry out rough flotation separation of the remaining bismuth and sulfur to obtain a bismuth-sulfur rough concentrate and a bismuth-sulfur flotation tailings;

[0036] S5, performing two closed-circuit pre-concentrations on the bismuth-sulfur coarse concentrate of step S4 to obtain a bismuth-sulfur mixed concentrate, and adding a slime inhibitor CD-N1 in both closed-circuit pre-concentration steps; performing bismuth-sulfur separation flotation on the bismuth-sulfur mixed concentrate to obtain a second bismuth concentrate and a sulfur concentrate;

[0037] S6. The bismuth-sulfur flotation tailings of step S4 are subjected to three closed-circuit scavenging processes to obtain final tailings, and the intermediate ores obtained in the three scavenging processes are returned to the previous process step by step.

[0038] In particular, the method is based on the commonality of the floatability of molybdenum, bismuth and sulfur minerals, and the mineral processing process is rationally designed to preferentially recover molybdenum and part of the bismuth with good floatability, and then recover the remaining bismuth and sulfur with poor floatability, and finally obtain the final molybdenum, bismuth and sulfur concentrates respectively through molybdenum-bismuth separation and bismuth-sulfur separation. The new mineral processing process scheme of the present invention effectively solves the interference of the large difference in floatability of bismuth minerals on the recovery and separation of molybdenum-bismuth-sulfur, and maximizes the avoidance of the problems of difficulty in separating molybdenum-bismuth-sulfur and poor indicators under the "molybdenum-bismuth-sulfur mixed floatation-molybdenum-bismuth-sulfur separation" process in the prior art and the low metal recovery rate under the "molybdenum-bismuth and other floatable-molybdenum-bismuth separation-tailings floating sulfur" process. By strengthening the mineral processing process in stages, the recovery efficiency and indicators of molybdenum, bismuth and sulfur mineral processing are improved, and the problem of efficient recovery and utilization of calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ores is solved.

[0039] Specifically, the components of the molybdenum-bismuth collector B11 include 40% to 50% of mineral oil, 30% to 40% of diesel, 10% to 20% of O-isopropyl-N-ethylthiocarbamate and 10% to 20% of polyoxypropylene ether by mass percentage; the molybdenum-bismuth collector system has good recovery of molybdenum and bismuth with high floatability through the synergistic coordination of various components. The foaming agent F9 includes 50% to 70% of triethoxybutyl ether, 20% to 30% of methyl isobutyl carbinol and 20% to 40% of camphor oil by mass percentage. The foaming agent has the advantages of strong foaming ability, good selectivity and stable foam layer through the synergistic coordination of various components. The slime inhibitor CD-N1 includes 40% to 50% hydroxyethyl cellulose, 10% to 30% locust bean gum and 20% to 30% lactic acid by mass percentage. Hydroxyethyl cellulose has a small molecular weight, good selectivity and weak inhibitory ability to metal ores, which makes the dosage of the slime inhibitor CD-N1 adjustable in a wide range. Locust bean gum and lactic acid can adjust the foam state, reduce the viscosity of the foam, make the gangue components fall off in the secondary enrichment process, and reduce the influence of gangue on the recovery rate of metal ore.

[0040] The present invention adopts a beneficiation process of partial preferential mixed flotation of molybdenum and bismuth-flotation of remaining bismuth and sulfur-separation of molybdenum and bismuth-bismuth sulfur, and recovers molybdenum and part of bismuth with good floatability through combined capture-foaming of reagents B11+F9. Through the reasonable selectivity of the collector system, the entrainment and flotation of calcium-magnesium muddy gangue is effectively avoided, and the rapid and efficient recovery of molybdenum and bismuth is achieved, while providing good molybdenum-bismuth mixed concentrate conditions for molybdenum-bismuth separation and flotation. At the same time, on the basis of using a strong collector, the reagent CD-N1 is used as an efficient calcium-magnesium gangue inhibitor, which effectively reduces the interference of calcium-magnesium muddy gangue on the flotation and concentration process of bismuth-sulfur minerals, and provides conditions for the full and efficient recovery of bismuth and sulfur.

[0041] In step S3, the middlings produced by the first closed-circuit pre-concentration are returned to the molybdenum-bismuth part of step S2 for preferential mixed flotation, and the middlings produced by the second closed-circuit pre-concentration are returned to the first closed-circuit pre-concentration. The amount of the slime inhibitor CD-N1 added in the first closed-circuit pre-concentration is 40-60 g / t, and the amount of the slime inhibitor CD-N1 added in the second closed-circuit pre-concentration is 10-30 g / t. Activated carbon is added to scrub and remove the medicine during the molybdenum-bismuth separation flotation, and sodium sulfide or sodium hydrosulfide is selected as the bismuth inhibitor. The process of molybdenum-bismuth separation flotation is a combination of one rough three, four, five, six fine two, three, four scavenging, the amount of activated carbon is 100-500 g / t, the amount of sodium sulfide is 200-8000 g / t, or the amount of sodium hydrosulfide is 100-6000 g / t.

[0042] In step S4, the addition amount of the slime inhibitor CD-N1 is 180-220 g / t, the activator is copper sulfate, the addition amount is 130-170 g / t, the collectors are butyl xanthate and ethyl thiocyanate, the addition amounts are 80-120 g / t and 10-30 g / t respectively, and the addition amount of the foaming agent F9 is 10-20 g / t.

[0043] In step S5, the middlings produced by the first closed-circuit pre-selection are returned to the flotation roughing of the remaining bismuth and sulfur in step S4, and the middlings produced by the second closed-circuit pre-selection are returned to the first closed-circuit pre-selection. The amount of the slime inhibitor CD-N1 added in the first closed-circuit pre-selection is 80-120 g / t, and the amount of the slime inhibitor CD-N1 added in the second closed-circuit pre-selection is 40-60 g / t. Activated carbon is added to scrub and remove the medicine during bismuth-sulfur separation and flotation, and lime and sodium humate are selected as sulfur inhibitors; the process of bismuth-sulfur separation and flotation is a combination of one roughing, two, three, four, five fines, two, three, four scavenging, the amount of activated carbon is 100-500 g / t, the amount of lime is 500-10000 g / t, and the amount of sodium humate is 20-300 g / t.

[0044] In step S6, 50-100 g / t of slime inhibitor CD-N1, 30-50 g / t of butyl xanthate and 2-7 g / t of frother F9 are added in the three closed-circuit sweeps, the intermediate ore from the first closed-circuit sweep is returned to the rough flotation of the remaining bismuth and sulfur in step S4, and the intermediate ore from the second and third closed-circuit sweeps is returned to the previous sweep in turn.

[0045] The present invention uses a reasonable segmented recovery process of molybdenum, bismuth and sulfur, and cooperates with independently developed reagents to efficiently capture metal ores and effectively regulate calcium-magnesium mudstone, so that the cost of using the reagent is low, the difficulty of separating molybdenum, bismuth and bismuth sulfur is small, the amount of ore circulation in the main process is small, and the process flow is highly stable. The method effectively solves the problem of efficient recovery of calcium-magnesium gangue-containing molybdenum, bismuth and sulfur polymetallic ores, has a simple and reliable process, and an efficient reagent system, and provides a new and effective method for the recovery of similar molybdenum, bismuth and sulfur resources.

[0046] Example 1

[0047] This embodiment provides a method for beneficiation and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore, comprising the following steps:

[0048] S1. The raw ore is crushed to -2 mm, and then the crushed ore is ground using a Φ240×90 mm conical ball mill to obtain a grinding product in which the mineral powder with a fineness of less than 0.074 mm accounts for 80% of the total mass, and water is added to the grinding product to a pulp concentration of 30%; wherein the grade of the raw ore is: Mo grade 0.092%, Bi grade 0.053%, S grade 2.03%; the content of calcite is 5%, the content of dolomite is 3%, the content of grossular garnet is 15%, the content of tremolite is 5%, the content of actinolite is 5%, and the content of diopside is 5%;

[0049] S2, adding 100 g / t of molybdenum-bismuth collector B11 and 30 g / t of frother F9 to the slurry obtained in step S1, and performing partial preferential mixed flotation of molybdenum-bismuth to obtain a molybdenum-bismuth mixed coarse concentrate and molybdenum-bismuth flotation tailings;

[0050] S3, the molybdenum-bismuth mixed coarse concentrate of step S2 is subjected to two closed-circuit pre-concentrations to obtain a molybdenum-bismuth mixed concentrate, the middlings produced by the first closed-circuit pre-concentration are returned to the molybdenum-bismuth part of step S2 for preferential mixed flotation, the middlings produced by the second closed-circuit pre-concentration are returned to the first closed-circuit pre-concentration, the addition amount of the slime inhibitor CD-N1 in the first closed-circuit pre-concentration is 50 g / t, and the addition amount of the slime inhibitor CD-N1 in the second closed-circuit pre-concentration is 20 g / t;

[0051] The molybdenum-bismuth mixed concentrate is subjected to molybdenum-bismuth separation flotation, and a one-rough three-fine three-sweep selection process is selected, and 300g / t of activated carbon is added for scrubbing and de-doping, and 5000g / t of sodium sulfide is selected as a bismuth inhibitor to obtain a molybdenum concentrate and a first bismuth concentrate;

[0052] S4, the molybdenum-bismuth flotation tailings of step S2 are sequentially added with 200 g / t of slime inhibitor CD-N1, 150 g / t of activator copper sulfate, collector (100 g / t of butyl xanthate + 20 g / t of ethyl thiocyanate) and 15 g / t of frother F9 to carry out flotation roughing of the remaining bismuth and sulfur to obtain a bismuth-sulfur rough concentrate and a bismuth-sulfur flotation tailings;

[0053] S5, the bismuth-sulfur coarse concentrate of step S4 is subjected to two closed-circuit pre-concentrations to obtain a bismuth-sulfur mixed concentrate, and the slime inhibitor CD-N1 is added in both closed-circuit pre-concentration processes; the middlings produced by the first closed-circuit pre-concentration are returned to the flotation roughing of the remaining bismuth and sulfur in step S4, and the middlings produced by the second closed-circuit pre-concentration are returned to the first closed-circuit pre-concentration, and the amount of the slime inhibitor CD-N1 added in the first closed-circuit pre-concentration is 100 g / t, and the amount of the slime inhibitor CD-N1 added in the second closed-circuit pre-concentration is 50 g / t;

[0054] The bismuth-sulfur mixed concentrate is subjected to bismuth-sulfur separation flotation, a one-roughing-two-fine-three-scavenging process is selected, and 300 g / t of activated carbon is added for scrubbing and de-doping, and 6000 g / t of lime and 150 g / t of sodium humate are selected as a sulfur inhibitor to obtain a second bismuth concentrate and a sulfur concentrate, and the second bismuth concentrate is combined with the first bismuth concentrate in step S3 to form a bismuth concentrate;

[0055] S6. The bismuth-sulfur flotation tailings of step S4 are subjected to three closed-circuit sweeps to obtain the final tailings. 80 g / t of slime inhibitor CD-N1, 40 g / t of butyl xanthate and 5 g / t of frother F9 are added in the three closed-circuit sweeps. The middlings from the first closed-circuit sweep are returned to the rough flotation of the remaining bismuth and sulfur in step S4, and the middlings from the second and third closed-circuit sweeps are returned to the previous sweeps in turn.

[0056] The components of the molybdenum bismuth collector B11 used in this embodiment include 45% mineral oil, 35% diesel, 10% O-isopropyl-N-ethylthiocarbamate and 10% polyoxypropylene ether by mass percentage; the foaming agent F9 includes 60% triethoxybutyl ether, 25% methyl isobutyl carbinol and 15% camphor oil by mass percentage; the slime inhibitor CD-N1 includes 50% hydroxyethyl cellulose, 20% locust bean gum and 30% lactic acid by mass percentage.

[0057] The grade and recovery rate of each ore obtained in Example 1 were tested, and the results are shown in the following table.

[0058] Table 1 Experimental data obtained in Example 1

[0059]

[0060] It can be seen from Table 1 that the molybdenum concentrate, bismuth concentrate and sulfur concentrate obtained by the recovery method of this embodiment have high grade and high recovery rate, and the metal content in the tailings is low, which shows that this method improves the recovery efficiency and index of molybdenum, bismuth and sulfur beneficiation by strengthening the beneficiation process in stages, and solves the problem of efficient recovery and utilization of calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ore.

[0061] Comparative Example 1

[0062] Comparative Example 1 provides a method for the beneficiation and recovery of a calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ore. Compared with Example 1, the difference lies in that a conventional "molybdenum-bismuth-sulfur mixed flotation-molybdenum-bismuth-sulfur separation" flotation process is adopted, and the experimental data obtained are shown in the table below.

[0063] Table 2 Experimental data obtained from comparative example 1

[0064]

[0065] It can be seen from Table 2 that the conventional "molybdenum, bismuth and sulfur mixed flotation-molybdenum, bismuth and sulfur separation" flotation process for metal recovery results in a low molybdenum, bismuth and sulfur recovery rate.

[0066] Comparative Example 2

[0067] Comparative Example 2 provides a method for recovering a calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore. Compared with Example 1, the difference is that no slime inhibitor CD-N1 is added in step S3, step S4, step S5 and step S6, and the rest is roughly the same as Example 1, which will not be repeated here. The experimental data obtained in Comparative Example 2 are shown in the following table.

[0068] Table 3 Experimental data obtained from comparative example 2

[0069]

[0070] It can be seen from Table 3 that when the slime inhibitor CD-N1 is not added, the molybdenum, bismuth and sulfur recovery rate and concentrate grade are low due to the interference of calcium-magnesium muddy gangue on the preferential mixed flotation of molybdenum and bismuth, molybdenum-bismuth flotation tailings, bismuth-sulfur mineral flotation and concentration process.

[0071] Comparative Example 3

[0072] Comparative Example 3 provides a method for recovering molybdenum-bismuth-sulfur polymetallic ore containing calcium-magnesium gangue. Compared with Example 1, the difference is that in step S2, conventional kerosene is used instead of molybdenum-bismuth collector B11, and the rest is roughly the same as Example 1, which will not be repeated here. The experimental data obtained in Comparative Example 3 are shown in the following table.

[0073] Table 4 Experimental data obtained by comparative example 3

[0074]

[0075] Comparative Example 4

[0076] Comparative Example 4 provides a method for recovering a calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore. Compared with Example 1, the difference is that in step S2, a conventional foaming agent 2 is used. # Oil (pine oil) replaces the foaming agent F9, and the rest is substantially the same as in Example 1, which will not be described in detail here. The experimental data obtained in Comparative Example 4 are shown in the table below.

[0077] Table 5 Experimental data obtained by comparative example 4

[0078]

[0079] It can be seen from Tables 4 and 5 that the conventional collector kerosene or conventional foaming agent 2 # Oil mainly affects the separation and recovery of molybdenum and bismuth. The grade and recovery rate of molybdenum concentrate and bismuth concentrate decrease, mainly because the selectivity of kerosene and 2# oil decreases, resulting in a higher mutual content of metal separation, thus affecting the grade and recovery rate of the concentrate.

[0080] In summary, the present invention provides a beneficiation and recovery method for calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ore. Based on the commonality of the floatability of molybdenum, bismuth and sulfur minerals, the beneficiation process is rationally designed to preferentially recover molybdenum and part of bismuth with good floatability, and then recover the remaining bismuth and sulfur with poor floatability. Finally, by molybdenum-bismuth separation and bismuth-sulfur separation, the final molybdenum, bismuth and sulfur concentrates are obtained respectively; the beneficiation process scheme of molybdenum-bismuth partial preferential mixed flotation-remaining bismuth and sulfur flotation-molybdenum-bismuth separation-bismuth-sulfur separation effectively solves the interference of the floatability difference part in bismuth minerals on the recovery and separation of molybdenum-bismuth-sulfur, and maximizes the avoidance of the problems of difficult separation of molybdenum-bismuth-sulfur and poor indicators under the "molybdenum-bismuth-sulfur mixed flotation-molybdenum-bismuth-sulfur separation" process in the prior art and the low metal recovery rate under the "molybdenum-bismuth and other floatable-molybdenum-bismuth separation-tailings flotation sulfur" process in the prior art. By strengthening the beneficiation process in stages, the beneficiation recovery efficiency and indicators of molybdenum, bismuth and sulfur are improved, and the problem of efficient recovery and utilization of calcium-magnesium gangue-containing molybdenum-bismuth-sulfur polymetallic ore is solved. The present invention reduces the interference of calcium-magnesium argillaceous gangue on the enrichment and separation process of molybdenum, bismuth and sulfur through the combined capture-foaming of reagent B11+F9 and the inhibition of calcium-magnesium argillaceous gangue minerals by CD-N1, and strengthens the beneficiation process in stages, thereby improving the beneficiation recovery efficiency and index of molybdenum, bismuth and sulfur. The method effectively solves the problem of efficient recovery of calcium-magnesium gangue-type molybdenum, bismuth and sulfur polymetallic ores, has a simple and reliable process, and an efficient reagent system, and provides a new and effective method for the recovery of similar molybdenum, bismuth and sulfur resources.

[0081] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for recovering calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore, characterized in that: The following steps are involved: S1. Crushing and grinding the raw ore to obtain a grinding product in which the ore powder with a fineness of less than 0.074 mm accounts for 78% to 83% of the total mass, and adding water to the grinding product to a pulp concentration of 30% to 35%; S2, adding molybdenum-bismuth collector B11 and frother F9 to the slurry obtained in step S1, and performing partial preferential mixed flotation of molybdenum-bismuth to obtain molybdenum-bismuth mixed coarse concentrate and molybdenum-bismuth flotation tailings; S3, subjecting the molybdenum-bismuth mixed coarse concentrate of step S2 to two closed-circuit pre-concentrations to obtain a molybdenum-bismuth mixed concentrate, wherein the slime inhibitor CD-N1 is added in both closed-circuit pre-concentration steps; subjecting the molybdenum-bismuth mixed concentrate to molybdenum-bismuth separation flotation to obtain a molybdenum concentrate and a first bismuth concentrate; S4, adding a slime inhibitor CD-N1, an activator, a collector and a frother F9 to the molybdenum-bismuth flotation tailings of step S2 in sequence to carry out flotation roughing of the remaining bismuth and sulfur to obtain a bismuth-sulfur rough concentrate and a bismuth-sulfur flotation tailings; S5, subjecting the bismuth-sulfur coarse concentrate of step S4 to two closed-circuit pre-concentrations to obtain a bismuth-sulfur mixed concentrate, wherein the slime inhibitor CD-N1 is added in both closed-circuit pre-concentration steps; subjecting the bismuth-sulfur mixed concentrate to bismuth-sulfur separation flotation to obtain a second bismuth concentrate and a sulfur concentrate; S6. The bismuth-sulfur flotation tailings of step S4 are subjected to three closed-circuit scavenging processes to obtain final tailings, and the intermediate ores obtained in the three scavenging processes are returned to the previous process step by step.

2. The method for mineral processing and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore according to claim 1, characterized in that: The components of the molybdenum-bismuth collector B11 include, by mass percentage, 40% to 50% of mineral oil, 30% to 40% of diesel, 10% to 20% of O-isopropyl-N-ethylthiocarbamate and 10% to 20% of polyoxypropylene ether; the foaming agent F9 includes, by mass percentage, 50% to 70% of triethoxybutyl ether, 20% to 30% of methyl isobutyl carbinol and 20% to 40% of camphor oil; the slime inhibitor CD-N1 includes, by mass percentage, 40% to 50% of hydroxyethyl cellulose, 10% to 30% of locust bean gum and 20% to 30% of lactic acid.

3. The method for mineral processing and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore according to claim 2, characterized in that: In step S2, the added amount of the molybdenum-bismuth collector B11 is 80-120 g / t, and the added amount of the foaming agent F9 is 20-40 g / t.

4. The method for mineral processing and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore according to claim 1, characterized in that: In step S3, the middlings produced in the first closed-circuit pre-concentration are returned to the molybdenum-bismuth part of step S2 for preferential mixed flotation, and the middlings produced in the second closed-circuit pre-concentration are returned to the first closed-circuit pre-concentration. The amount of the slime inhibitor CD-N1 added in the first closed-circuit pre-concentration is 40-60 g / t, and the amount of the slime inhibitor CD-N1 added in the second closed-circuit pre-concentration is 10-30 g / t. During the molybdenum-bismuth separation flotation, activated carbon is added for scrubbing and drug removal, and sodium sulfide or sodium hydrosulfide is selected as the bismuth inhibitor.

5. The method for mineral processing and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore according to claim 1, characterized in that: In step S4, the added amount of the slime inhibitor CD-N1 is 180-220 g / t, the activator is copper sulfate, and the added amount is 130-170 g / t, the collectors are butyl xanthate and ethyl thiocyanate, and the added amounts are 80-120 g / t and 10-30 g / t respectively, and the added amount of the foaming agent F9 is 10-20 g / t.

6. The method for mineral processing and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore according to claim 1, characterized in that: In step S5, the middlings produced in the first closed-circuit pre-concentration are returned to the flotation roughing of the remaining bismuth and sulfur in step S4, and the middlings produced in the second closed-circuit pre-concentration are returned to the first closed-circuit pre-concentration. The amount of the slime inhibitor CD-N1 added in the first closed-circuit pre-concentration is 80-120 g / t, and the amount of the slime inhibitor CD-N1 added in the second closed-circuit pre-concentration is 40-60 g / t; activated carbon is added for scrubbing and removing the drug during the bismuth-sulfur separation flotation, and lime and sodium humate are selected as the sulfur inhibitor.

7. The method for mineral processing and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore according to claim 1, characterized in that: In step S6, 50-100 g / t of slime inhibitor CD-N1, 30-50 g / t of butyl xanthate and 2-7 g / t of frother F9 are added to the three closed-circuit sweeps, the middlings from the first closed-circuit sweep are returned to the rough flotation of the remaining bismuth and sulfur in step S4, and the middlings from the second and third closed-circuit sweeps are returned to the previous sweeps in turn.

8. The method for mineral processing and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore according to claim 4, characterized in that: The molybdenum-bismuth separation flotation process is a combination of one coarse three, four, five, six fine two, three, four scavenging, the amount of activated carbon used is 100-500g / t, the amount of sodium sulfide used is 200-8000g / t, or the amount of sodium hydrosulfide used is 100-6000g / t.

9. The method for mineral processing and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore according to claim 6, characterized in that: The bismuth-sulfur separation flotation process is a combination of one coarse, two, three, four, five fine, two, three, four scavenging, the amount of activated carbon used is 100-500g / t, the amount of lime used is 500-10000g / t, and the amount of sodium humate used is 20-300g / t.

10. The method for mineral processing and recovery of calcium-magnesium gangue-type molybdenum-bismuth-sulfur polymetallic ore according to claim 1, characterized in that: In step S1, the grade of the ore is: Mo grade 0.05%-0.15%, Bi grade 0.05%-0.2%, S grade 0.5%-4.5%; the content of calcite is 2%-8%, the content of dolomite is 0.5%-5%, the content of grossular garnet is 10%-25%, the content of tremolite is 1%-10%, the content of actinolite is 1%-10%, and the content of diopside is 1%-10%.

Citation Information

Patent Citations

  • Beneficiation method for cascade enhanced flotation and efficient recovery of low-grade molybdenum-bismuth-sulfur polymetallic ore

    CN115780069A

  • Beneficiation method for flotation and efficient recovery of low-grade molybdenum-bismuth-sulfur polymetallic ore

    CN117046613A

  • Flotation agent, and molybdenum bismuth sulfur multi-metal ore flotation selection separation method

    CN110237938A

  • Efficient non-toxic molybdenum, bismuth and sulfur recovery method

    CN114192286A

  • Beneficiation method for tungsten-tin multi-metal ore containing copper, molybdenum and bismuth