Self-lubricating coating based on titanium alloy surface texture and preparation method thereof
By preparing MoS2 composite crystallization and laser texture treatment on the surface of titanium alloy, combined with air spraying, the stability and functional consistency of the titanium alloy surface coating in harsh environments is solved, and high-efficiency and low-cost self-lubricating is achieved Coating preparation significantly improves wear resistance and friction reduction performance.
Patent Information
- Application Number
- CN202411178976.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to ensure the long-term stability and functional consistency of the titanium alloy surface coating under harsh environments, and the preparation process is complex and costly.
By mixing molybdenum disulfide (MoS2) with tetrahydrofuran and acetylanilide, adding dimethyl sulfoxide, uniform MoS2 composite crystals were prepared, and combined with laser texture treatment and air spraying, a titanium alloy surface texture was prepared. Self-lubricating coating.
It significantly improves the uniformity and adhesion of the coating, ensures long-term stability and functional consistency in harsh environments, simplifies the process flow, reduces the preparation cost, and significantly improves wear resistance and friction reduction performance.
Smart Images

Figure CN119056723A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface engineering, and in particular to a self-lubricating coating based on titanium alloy surface texture and a preparation method thereof. Background Art
[0002] Titanium alloys are widely used in high-tech fields such as aerospace, medical equipment and automobile manufacturing due to their excellent mechanical properties, corrosion resistance and high specific strength. However, despite their obvious advantages in high strength and lightweight, their inherent low friction properties have become one of the main obstacles to their further development. High friction conditions will make titanium alloys prone to severe surface wear, leading to material failure and shortened component service life. Bionic texture technology has significantly improved the friction reduction and wear resistance of titanium alloy surfaces, but texture structures are often prone to wear or failure under complex environments such as high loads and high corrosion. It is difficult to maintain excellent friction reduction and wear resistance for a long time relying solely on texture. Therefore, the preparation of self-lubricating and wear-resistant coatings on textured surfaces has become an important means to improve the tribological properties of key service components.
[0003] Traditional self-lubricating coating technology usually introduces solid lubricants, such as molybdenum disulfide (MoS2), on the surface of the substrate to achieve a significant reduction in the friction coefficient and an improvement in wear resistance. However, in practice, it is difficult to effectively and evenly deposit MoS2 on the surface of titanium alloys, and the coating maintains stability, durability and excellent mechanical properties during long-term use, which is still a technical problem that needs to be solved in the field of material surface engineering. The existing MoS2 coating preparation method usually relies on a multi-step complex process, and the lubricating coating is prepared by chemical vapor deposition (CVD), physical vapor deposition (PVD) and electrochemical deposition, thereby improving its bonding force and tribological properties. For example, the document with application number "CN109161870A" discloses "a nano-textured atomic layer deposition molybdenum disulfide soft coating tool and its preparation method", and its nano-textured atomic layer deposition molybdenum disulfide soft coating tool is prepared by the process of high-energy beam processing texture and atomic layer deposition coating. Although this method can achieve the deposition of MoS2 to a certain extent, its process is complex, the equipment requirements are high, the manufacturing cost is relatively high, and the resulting coating still has significant deficiencies in bonding strength, thickness uniformity and wear resistance. It is difficult to ensure the long-term stability and functional consistency of the coating under harsh environments, resulting in great restrictions on its promotion in actual engineering applications.
[0004] The existing MoS2 coating preparation method also uses composite metal materials to prepare lubricating coatings. For example, the document with application number "CN202110173462.3" discloses "a kind of lubricating and wear-resistant composite coating prepared on the surface of aviation aluminum alloy", which uses constant voltage DC anodizing to prepare a regular porous alumina nanopore array on the surface of aviation aluminum alloy, and then co-deposits molybdenum disulfide and metal tungsten by radio frequency sputtering and DC sputtering to form an AAO / MoS2-W composite reinforced lubricating layer. However, it requires the use of a constant voltage DC power supply, radio frequency and DC sputtering equipment, which increases economic and time costs, and requires strict control of process parameters such as temperature, atmosphere, deposition rate, etc., and the process complexity is high. Summary of the invention
[0005] The present invention provides a self-lubricating coating based on titanium alloy surface texture and a preparation method thereof to solve the problems existing in the prior art that it is difficult to ensure the long-term stability and functional consistency of the coating under harsh environments, the equipment is expensive, and long-term professional operation is required, and the process is highly complex.
[0006] To achieve the above object, the technical solution of the present invention is as follows: A method for preparing a self-lubricating coating based on titanium alloy surface texture, comprising the following steps:
[0007] Step 1, preparing molybdenum disulfide (MoS2) composite crystals: Molybdenum disulfide and tetrahydrofuran are mixed in a certain amount of deionized water and ethanol, stirred, and then acetanilide is added. After continuing to stir evenly, stirring at room temperature until the solution precipitates white crystals, filtering and drying for standby use, to obtain molybdenum disulfide (MoS2) composite crystals;
[0008] Step 2: dispersing molybdenum disulfide (MoS2) composite crystals and additives in anhydrous ethanol according to a certain mass ratio to prepare a mixed coating;
[0009] Step 3: deposit the mixed coating onto the pretreated titanium alloy material substrate, and after drying and curing, prepare a self-lubricating coating based on the surface texture of the titanium alloy.
[0010] Furthermore, in the above step 1, the mass ratio of molybdenum disulfide (MoS2), tetrahydrofuran (THF) and acetanilide is 4:1-2:1-2.
[0011] Furthermore, in the above step 1, the stirring temperature is 40-60°C for 20-40 minutes; the stirring temperature is continued at 40-60°C for 20-40 minutes.
[0012] Furthermore, in the above step 2, the mass ratio of molybdenum disulfide (MoS2) composite crystals and additives is 15:1-3.
[0013] Furthermore, in the above step 2, the additive is dimethyl sulfoxide (DMSO).
[0014] Furthermore, in the above step 2, the preferred mass ratio of the molybdenum disulfide (MoS2) composite crystal and the additive is 15:2.
[0015] Furthermore, in the above step 3, the titanium alloy material substrate is pretreated, and the process includes:
[0016] The titanium alloy sample was ground and polished, ultrasonically washed with acetone and ethanol in turn, and then dried. It was then laser texturing treated by adjusting the laser power to 3W and the scanning speed to 6mm / s. A serrated texture imitating the shark skin texture with different area densities was prepared on the surface of the substrate. It was heated at 150°C for 0.5h and then set aside.
[0017] Furthermore, in the above step three, the mixed coating is deposited using an air spraying method, with a spray gun nozzle diameter of 0.8 mm and a spray gun air pressure of 0.35 MPa.
[0018] Furthermore, the above preparation method produces a self-lubricating coating based on the surface texture of the titanium alloy.
[0019] Compared with the prior art, the advantages of the present invention are:
[0020] 1. The present invention dissolves molybdenum disulfide (MoS2) and tetrahydrofuran (THF) in deionized water and ethanol, adds acetanilide as a cosolvent to avoid agglomeration, and then adds dimethyl sulfoxide (DMSO) to enhance surface binding force, thereby effectively improving the uniformity and chemical activity of the MoS2 solution. Dimethyl sulfoxide (DMSO) and tetrahydrofuran work together to enhance the uniformity of the solution, thereby achieving uniform deposition on the titanium alloy surface and significantly enhancing the adhesion of the coating. The long-term stability and functional consistency of the coating can be guaranteed under harsh environments.
[0021] 2. The present invention greatly simplifies the process flow and improves production efficiency: not only environmentally friendly solvents and additives are used in the preparation process to reduce the requirements for the operating environment and reduce the emission of harmful gases, but also air spraying and laser texturing are implemented on the titanium alloy substrate, the process simplification effect is good, the texture has a significant improvement in the adhesion of the coating, and the coating can be stored and the lubricating medium can be continuously output to the outside. By combining the synergistic effect of surface texture and self-lubricating coating, the wear resistance and tribological properties of the coating are significantly improved. Especially in high friction and high load environments, the coating provided by the present invention exhibits excellent durability and stability, and its friction reduction performance and wear resistance are greatly improved.
[0022] 3. The invention has a wide range of applications: The method of the invention has good adaptability and operability, and can efficiently prepare self-lubricating coatings on titanium alloy substrates of various shapes and sizes. The drying and curing process of the coating ensures the density and performance consistency of the coating, and the preparation cost is low. The prepared coating has excellent lubrication effect under complex working conditions and can be used for lubrication and protection of bearings, guide rails, sliders and other components, and can meet the needs of different industrial application fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a microscopic image of the lubricating coating prepared on the textured surface;
[0024] Figure 2 is the friction coefficient curve of the coating made of 10% area density and 10g of the additive dimethyl sulfoxide in Example 1;
[0025] Figure 3 is the friction coefficient curve of the coating made of 14% area density and 20g of dimethyl sulfoxide additive in Example 2;
[0026] Figure 4 is the friction coefficient curve of the coating made of 18% area density and 30g of dimethyl sulfoxide additive in Example 3;
[0027] Figure 5 is a graph showing the wear amount of coatings made of different area densities and different contents of the additive dimethyl sulfoxide in Examples 1, 2, and 3;
[0028] Figure 6 The SEM and EDS elemental surface scans of the coating made of 10% area density and 10g of dimethyl sulfoxide additive in Example 1;
[0029] Figure 7 The SEM and EDS elemental surface scans of the coating made of 14% area density and 20g of dimethyl sulfoxide additive in Example 2;
[0030] Figure 8 These are the SEM and EDS elemental surface scans of the coating made with 18% area density and 30g of dimethyl sulfoxide as an additive in Example 3. DETAILED DESCRIPTION
[0031] The present invention will be further described below in conjunction with specific embodiments and accompanying drawings.
[0032] The present invention uses titanium alloy as a substrate, processes surface texture, and prepares a self-lubricating coating at the same time. The coating is prepared by dissolving molybdenum disulfide (MoS2) and tetrahydrofuran (THF) into deionized water and ethanol, introducing acetanilide, and then adding dimethyl sulfoxide (DMSO). Laser texturing is performed on the titanium alloy substrate to form a tooth-like texture imitating shark skin texture with different area densities, and then air spraying is performed to obtain a self-lubricating coating.
[0033] Unless otherwise specified, the materials and reagents used in the present invention are all conventional reagents and can be purchased on the market; the methods used are all conventional methods unless otherwise specified.
[0034] Embodiment 1, a method for preparing a self-lubricating coating based on titanium alloy surface texture, comprising the following steps:
[0035] Step 1: Preparation of MoS2 composite crystals:
[0036] In a stirred reaction vessel, gradually add 100g of molybdenum disulfide (MoS2) powder to a mixed solution of 100ml of deionized water and 200ml of ethanol, stir gently to initially disperse the powder, and slowly add 25g Tetrahydrofuran (THF), ensure that the solution is stirred evenly during the addition process to allow molybdenum disulfide to fully contact tetrahydrofuran. Heat the reaction vessel to 40°C and continue stirring at this temperature for 20 minutes to ensure that molybdenum disulfide is evenly dispersed in the solution, then gradually add 25g of acetanilide while maintaining 40°C, and continue stirring for 20 minutes to promote the chemical reaction. Continue stirring at room temperature until white crystals precipitate, separate the white crystals through a filter, and dry them in a dryer to obtain molybdenum disulfide composite crystals.
[0037] Step 2, preparing mixed coating;
[0038] Prepare 150g of molybdenum disulfide composite crystals and 10g of additive dimethyl sulfoxide (DMSO), pour 200ml of anhydrous ethanol into a clean stirring container, gradually add the molybdenum disulfide composite crystals, and stir slowly; gradually add dimethyl sulfoxide, and continue stirring for 20 minutes to obtain a mixed coating.
[0039] Step 3: Deposit the mixed coating onto the base titanium alloy material to prepare a self-lubricating coating based on the surface texture of the titanium alloy:
[0040] First, a disc-shaped titanium alloy sample was prepared, and it was polished with 240-2000 grit sandpaper to make the surface smooth and burr-free, and then finely polished with flannel.
[0041] The sample was then ultrasonically cleaned in acetone and ethanol in turn to remove surface residues, and then laser texturing was performed using a laboratory-grade femtosecond laser system FemtoLAB. The laser power was set to 3W and the scanning speed was set to 6mm / s. A shark skin-like tooth-like texture with an area density of 10% was formed on the surface. The sample was then heated at 150°C for 20 minutes.
[0042] Afterwards, use Anest Iwata W-400 spray gun to evenly spray the mixed coating on the surface of the substrate by air spraying. The nozzle diameter of the spray gun is 0.8 mm, and the air pressure is set to 0.35 MPa. Keep the spray gun perpendicular to the substrate surface during spraying, at a distance of about 20 cm, and spray from left to right 5 times to ensure that the coating covers and penetrates the texture layer to complete the formation of the liquid coating. The coating is then placed in an oven and dried at 200°C for 1 hour to evaporate the ethanol and retain the lubricating phase in the texture pits.
[0043] Finally, the coating was pressure-polished using 2000-grit sandpaper and flannel cloth. The polishing machine speed was set to 5000 r / min and a load of 20 N was applied to ensure the density of the coating. The coating was cured at 300 °C for 1 h to prepare a lubricating coating with high friction reduction and wear resistance.
[0044] Embodiment 2, a method for preparing a self-lubricating coating based on titanium alloy surface texture, comprising the following steps:
[0045] Step 1: Preparation of MoS2 composite crystals:
[0046] In a stirred reaction vessel, 100g of molybdenum disulfide (MoS2) powder is gradually added to a mixed solution of 100ml of deionized water and 200ml of ethanol, gently stirred to preliminarily disperse the powder, and 35g of tetrahydrofuran (THF) is slowly added to ensure that the solution is uniformly stirred during the addition process so that molybdenum disulfide and tetrahydrofuran are fully in contact. The reaction vessel is heated to 50°C, and stirred continuously for 30mins at this temperature to ensure that molybdenum disulfide is uniformly dispersed in the solution, and then 35g of acetanilide is gradually added under the condition of maintaining 50°C, and stirring is continued for 30mins to promote the chemical reaction. Stirring is continued at room temperature until white crystals are precipitated, white crystals are separated by a filter, and are placed in a dryer for drying to obtain molybdenum disulfide composite crystals.
[0047] Step 2, preparing mixed coating;
[0048] Prepare 150g of molybdenum disulfide composite crystals and 20g of additive dimethyl sulfoxide (DMSO), pour 200ml of anhydrous ethanol into a clean stirring container, gradually add the molybdenum disulfide composite crystals while stirring slowly; gradually add dimethyl sulfoxide and continue stirring for 30 minutes to obtain a mixed coating. If necessary, the stirring time can be appropriately extended to ensure that the solution is completely uniform.
[0049] Step 3: Deposit the mixed coating onto the base titanium alloy material to prepare a self-lubricating coating based on the surface texture of the titanium alloy:
[0050] First, a disc-shaped titanium alloy sample was prepared, and it was polished with 240-2000 grit sandpaper to make the surface smooth and burr-free, and then finely polished with flannel.
[0051] The sample was then ultrasonically cleaned in acetone and ethanol in turn to remove surface residues, and then laser texturing was performed using a laboratory-grade femtosecond laser system FemtoLAB. The laser power was set to 3W and the scanning speed was set to 6mm / s. A shark skin-like tooth-like texture with an area density of 14% was formed on the surface. The sample was then heated at 150°C for 30 minutes.
[0052] After that, the mixed coating was evenly sprayed on the substrate surface using an Anest Iwata W-400 spray gun with an air spray method. The nozzle diameter of the spray gun was 0.8 mm, and the air pressure was set to 0.35 MPa. The spray gun was kept perpendicular to the substrate surface at a distance of about 20 cm. The coating was sprayed from left to right 5 times to ensure that the coating covered and penetrated the texture layer to complete the formation of the liquid coating. The coating was then placed in an oven and dried at 200 ° C for 1 h to evaporate the ethanol and retain the lubricating phase in the texture pits.
[0053] Finally, the coating was pressure-polished using 2000-grit sandpaper and flannel cloth. The polishing machine speed was set to 5000 r / min and a load of 20 N was applied to ensure the density of the coating. The coating was cured at 300 °C for 1 h to prepare a lubricating coating with high friction reduction and wear resistance.
[0054] Embodiment 3, a method for preparing a self-lubricating coating based on titanium alloy surface texture, comprising the following steps:
[0055] Step 1: Preparation of MoS2 composite crystals:
[0056] In a stirred reaction vessel, 100g of molybdenum disulfide (MoS2) powder is gradually added to a mixed solution of 100ml of deionized water and 200ml of ethanol, gently stirred to preliminarily disperse the powder, and 50g of tetrahydrofuran (THF) is slowly added to ensure that the solution is uniformly stirred during the addition process so that molybdenum disulfide and tetrahydrofuran are fully in contact. The reaction vessel is heated to 60°C, and stirred continuously for 40mins at this temperature to ensure that molybdenum disulfide is uniformly dispersed in the solution, and then 50g of acetanilide is gradually added while maintaining 60°C, and stirring is continued for 40mins to promote the chemical reaction. Stirring is continued at room temperature until white crystals are precipitated, white crystals are separated by a filter, and are placed in a dryer for drying to obtain molybdenum disulfide composite crystals.
[0057] Step 2, preparing mixed coating;
[0058] Prepare 150g of molybdenum disulfide composite crystals and 30g of additive dimethyl sulfoxide (DMSO), pour 200ml of anhydrous ethanol into a clean stirring container, gradually add the molybdenum disulfide composite crystals while stirring slowly; gradually add dimethyl sulfoxide and continue stirring for 40mins to obtain a mixed coating. If necessary, the stirring time can be appropriately extended to ensure that the solution is completely uniform.
[0059] Step 3: Deposit the mixed coating onto the base titanium alloy material to prepare a self-lubricating coating based on the surface texture of the titanium alloy:
[0060] First, a disc-shaped titanium alloy sample was prepared, and it was polished with 240-2000 grit sandpaper to make the surface smooth and burr-free, and then finely polished with flannel.
[0061] The sample was then ultrasonically cleaned in acetone and ethanol in turn to remove surface residues, and then laser texturing was performed using a laboratory-grade femtosecond laser system FemtoLAB. The laser power was set to 3W and the scanning speed was set to 6mm / s. A shark skin-like tooth-like texture with an area density of 18% was formed on the surface. The sample was then heated at 150°C for 40 minutes.
[0062] Afterwards, use Anest Iwata W-400 spray gun to evenly spray the mixed coating on the surface of the substrate by air spraying. The nozzle diameter of the spray gun is 0.8 mm, and the air pressure is set to 0.35 MPa. Keep the spray gun perpendicular to the substrate surface during spraying, at a distance of about 20 cm, and spray from left to right 5 times to ensure that the coating covers and penetrates the texture layer to complete the formation of the liquid coating. The coating is then placed in an oven and dried at 200°C for 1 hour to evaporate the ethanol and retain the lubricating phase in the texture pits.
[0063] Finally, the coating was pressure-polished using 2000-grit sandpaper and flannel cloth. The polishing machine speed was set to 5000 r / min and a load of 20 N was applied to ensure the density of the coating. The coating was cured at 300 °C for 1 h to prepare a lubricating coating with high friction reduction and wear resistance.
[0064] Table 1 is the comparison results of average friction coefficient and wear loss under different contents of tetrahydrofuran, acetanilide, additive dimethyl sulfoxide (DMSO), different texture area density and texture sample heating time.
[0065] Example unit Example 1 Example 2 Example 3 Dimethyl sulfoxide g 10 20 30 Texture area density / 10% 14% 18% Tetrahydrofuran g 25 35 50 Acetanilide g 25 35 50 Stirring time min 20 30 40 Texture sample heating time min 20 30 40 Average friction coefficient / 0.131 0.095 0.152 Wear <![CDATA[mm 3 ]]> 2.531 0.954 1.848
[0066] In order to further illustrate the tribological performance provided by the present invention, relevant tests were carried out on the embodiments, which are described in conjunction with the accompanying drawings, as follows:
[0067] The friction coefficient was evaluated using a reciprocating friction and wear testing machine with a load of 8N, a dual ball of CGr15 bearing steel ball, a friction reciprocating stroke of 6mm, and a friction speed of 10mm / s.
[0068] Figure 2 , Figure 5 , Figure 6 1 is a related drawing in Example 1, Figure 2 The friction curve shows that the texturing treatment and lubricating coating enhancement effect of the present invention reduce the friction coefficient by 60.6% compared to 0.331 of the untreated surface, and it is relatively stable. Figure 5 The wear volume is 91.05% lower than that of the untreated surface, which is only 2.531 mm 3 . Figure 6 The SEM image shows that there are many plowing phenomena and some wear particles. The element distribution map shows that the lubricating phase is filled in the texture pits, and the Mo and S elements are distributed more.
[0069] Figure 3 , Figure 5 , Figure 7 2 are the related drawings in Example 2, Figure 3 The friction curve shows that the texturing treatment and lubricating coating enhancement effect of the present invention reduce the friction coefficient by 71.2% compared to 0.331 of the untreated surface, and it is very stable. Figure 5 The wear volume is 96.63% lower than that of the untreated surface, which is only 0.095mm 3 . Figure 7 The SEM image shows that there is almost no plowing phenomenon and very few wear particles. The element distribution map shows that the lubricating phase is filled in the texture pits, and Mo and S elements are the most distributed.
[0070] Figure 4 , Figure 5 , Figure 8 3 is a related figure in Example 3, Figure 4 The friction curve shows that the texturing treatment and lubricating coating enhancement effect of the present invention reduce the friction coefficient by 53.9% compared to 0.331 of the untreated surface, and it is relatively stable. Figure 5 The wear volume is 93.46% lower than that of the untreated surface, which is only 1.848 mm. 3 . Figure 8 The SEM image shows that there are many plowing phenomena and some wear particles. The element distribution map shows that the lubricating phase is filled in the texture pits, and the Mo and S elements are distributed more.
[0071] In summary, embodiment 2 is the best embodiment.
[0072] Although the embodiments of the present invention have been listed above, it should be understood that these embodiments are only for explanation and not for limiting the scope of the present invention. Those skilled in the art may make various modifications, equivalent substitutions and improvements without departing from the spirit and scope of the present invention.
Claims
1. A method for preparing a self-lubricating coating based on titanium alloy surface texture, characterized in that: The following steps are involved: Step 1, preparing molybdenum disulfide (MoS2) composite crystals: mixing molybdenum disulfide and tetrahydrofuran into a certain amount of deionized water and ethanol, stirring, then adding acetanilide, continuing to stir evenly, stirring at room temperature until white crystals precipitate from the solution, filtering and drying for later use, to obtain molybdenum disulfide (MoS2) composite crystals; Step 2: dispersing molybdenum disulfide (MoS2) composite crystals and additives in anhydrous ethanol according to a certain mass ratio to prepare a mixed coating; Step 3: deposit the mixed coating onto the pretreated titanium alloy material substrate, and after drying and curing, prepare a self-lubricating coating based on the surface texture of the titanium alloy.
2. The method for preparing a self-lubricating coating based on titanium alloy surface texture according to claim 1, characterized in that: In the step 1, the mass ratio of molybdenum disulfide (MoS2), tetrahydrofuran (THF) and acetanilide is 4:1-2:1-2.
3. The method for preparing a self-lubricating coating based on titanium alloy surface texture according to claim 2, characterized in that: In the step 1, the stirring temperature is 40-60°C for 20-40 minutes; the stirring temperature is continued at 40-60°C for 20-40 minutes.
4. The method for preparing a self-lubricating coating based on titanium alloy surface texture according to claim 3, characterized in that: In the step 2, the mass ratio of the molybdenum disulfide (MoS2) composite crystal to the additive is 15:1-3.
5. The method for preparing a self-lubricating coating based on titanium alloy surface texture according to claim 4, characterized in that: In the step 2, the additive is dimethyl sulfoxide (DMSO).
6. The method for preparing a self-lubricating coating based on titanium alloy surface texture according to claim 5, characterized in that: In the step 2, the preferred mass ratio of the molybdenum disulfide (MoS2) composite crystal and the additive is 15:
2.
7. The method for preparing a self-lubricating coating based on titanium alloy surface texture according to claim 1, characterized in that: In the step 3, the titanium alloy material substrate is pretreated, and the process includes: The titanium alloy sample was ground and polished, ultrasonically washed with acetone and ethanol in turn, and then dried. It was then laser texturing treated by adjusting the laser power to 3W and the scanning speed to 6mm / s. A serrated texture imitating the shark skin texture with different area densities was prepared on the surface of the substrate. It was heated at 150°C for 0.5h and then set aside.
8. The method for preparing a self-lubricating coating based on titanium alloy surface texture according to claim 7, characterized in that: In the step three, the mixed coating is deposited by air spraying, the diameter of the spray gun is 0.8 mm, and the air pressure of the spray gun is 0.35 MPa.
9. The self-lubricating coating based on titanium alloy surface texture obtained by the preparation method according to claim 1.