Control method for avoiding folding defect during rotary swaging machining of alloy bar
Through the full-process optimization method, the folding defects in alloy rod rotary forging are solved, the processing quality and efficiency are improved, and the high performance and long life of the product are ensured.
Patent Information
- Application Number
- CN202411163019.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
AI Technical Summary
Common folding defects in alloy rod rotary forging are mainly caused by unreasonable mold design, uneven metal distribution and poor lubrication, and uneven metal deformation and sharp changes caused by improper operation.
The full process optimization from the design stage to inspection and quality control includes material selection and pretreatment, mold design optimization, precise heating process control, online monitoring and adjustment, annealing and surface treatment, as well as non-destructive testing and rigorous dimensional and performance testing , ensure the rationality of materials and molds and the stability of the processing process.
It significantly improves the quality and efficiency of alloy rod rotary forging processing, prevents folding defects, improves the mechanical properties, corrosion resistance and aesthetics of the product, meets the strict requirements of high-quality alloy products, and extends the service life of the product.
Smart Images

Figure CN119056985A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rotary forging methods, and in particular relates to a control method for avoiding folding defects during rotary forging of alloy rods. Background Art
[0002] Alloy bar rotary forging is a processing technology that uses a rotary forging press, also known as rotary forging or radial forging. Rotary forging is a forging mechanical process that combines forging and rolling. It uses high-frequency radial reciprocating motion to strike the workpiece, so that the workpiece can achieve radial compression and length extension deformation during the process of rotation and axial movement. This process is widely used in the processing of various alloy bars, especially high-strength and low-plasticity alloy materials such as tungsten, molybdenum, niobium, etc. Rotary forging is widely used in the processing of various alloy bars, especially in the manufacturing industries such as automobiles, tractors, machine tools, locomotives, etc., for the production of complex-shaped parts such as stepped shafts, hollow shafts, and inner wall profiles.
[0003] The folding defect that occurs during the rotary forging of alloy rods is a common problem that needs to be taken seriously during the metal forming process. Folding defects may occur during the rotary forging of alloy rods due to unreasonable die design, uneven metal distribution, poor lubrication and improper operation. Folding defects are formed when the oxidized surface metal merges together during the metal deformation process. It can be formed by the confluence of two (or more) strands of metal, or by the rapid and large flow of a metal that carries the surface metal of the adjacent part with it, and the two merge. In addition, folding may also be caused by bending and reflow of the deformed metal, or by partial deformation of part of the metal being pressed into another part of the metal. In order to prevent the occurrence of folding defects, it is necessary to make certain improvements to the current process of rotary forging of alloy rods. Summary of the invention
[0004] The object of the present invention is to provide a control method for avoiding folding defects during rotary forging of alloy rods, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to achieve the above object, the present invention provides the following technical solution: a control method for avoiding folding defects during rotary forging of alloy rods, comprising the following steps:
[0006] S1: Design stage;
[0007] S2: processing stage;
[0008] S3 post-processing stage;
[0009] S4: Inspection and quality control;
[0010] The design stage includes material selection, material pretreatment, mold material selection, and mold design optimization. The material pretreatment includes material cleaning and material heating. The mold material selection includes finite element analysis, mold geometry design, and cooling channel design. The processing stage includes heating process, rotary forging process, online monitoring and adjustment. The heating process includes heating equipment, heating temperature, heating time, and temperature uniformity. The rotary forging process includes forging temperature, forging speed, pressure control, rotation speed, and forging time. The online monitoring and adjustment includes process monitoring, data acquisition, and automatic adjustment. The post-processing stage includes annealing and surface treatment. The annealing includes annealing temperature, annealing time, and cooling method. The surface treatment includes surface polishing and coating treatment. The inspection and quality control include non-destructive testing and size and performance testing.
[0011] As a further technical solution of the present invention, the material selection includes determining the specific composition of the alloy, and the alloy is preferably selected from aluminum alloy, titanium alloy, and nickel-based alloy. The aluminum alloy adopts the 7075 series, the titanium alloy adopts Ti-6Al-4V, and the nickel-based alloy adopts Inconel 718. It is necessary to select a suitable alloy according to the mechanical properties, high temperature resistance and flow characteristics of the material. When cleaning the material, a sulfuric acid-hydrofluoric acid mixed solution is used to clean the material for 5-10 cleaning times. After cleaning, the material is rinsed with deionized water for 3-5 minutes. The material heating needs to set different heating parameters according to different alloys, wherein the aluminum alloy needs to be heated to 450-500°C and maintained for 15-30 minutes, the titanium alloy needs to be heated to 800-900°C and maintained for 30-60 minutes, and the nickel-based alloy needs to be heated to 1100-1200°C and maintained for 30-60 minutes.
[0012] As a further technical solution of the present invention, the mold material is H13 steel and tungsten alloy, the finite element analysis includes using FEA software for simulation, analyzing alloy flow and stress distribution, adjusting the mold design, and ensuring uniform material flow, the mold geometry includes a transition angle not exceeding 10°, and avoiding sharp changes, and the runner design adopts a progressive contraction design, the runner diameter is 20-30mm, and the width is 5-10mm, and the cooling channel design includes evenly distributing the cooling channels in key areas of the mold, and the channel diameter is controlled at 6-8mm.
[0013] As a further technical solution of the present invention, the heating equipment includes an induction heating resistance furnace, and the frequency is 100-200kHz, the power is 10-20kW, and the temperature control accuracy is ±5°C. The heating temperature corresponds to the temperature of each alloy: aluminum alloy: 450-500°C, titanium alloy: 800-900°C, and nickel-based alloy: 1100-1200°C. The heating time corresponds to the time of each alloy: aluminum alloy is controlled at 15-30 minutes, titanium alloy is controlled at 30-60 minutes, and nickel-based alloy is controlled at 30-60 minutes. The temperature uniformity includes using at least four temperature sensors to control the temperature fluctuation within ±10°C.
[0014] As a further technical solution of the present invention, the forging temperatures of the various alloys are 400-500°C for aluminum alloys, 850-900°C for titanium alloys, and 1150-1200°C for nickel-based alloys. The forging speeds corresponding to the speeds of the various alloys are 5-10 mm / s for aluminum alloys, 2-5 mm / s for titanium alloys, and 1-3 mm / s for nickel-based alloys. The pressures controlled corresponding to the pressures of the various alloys are 2000-4000 kN for aluminum alloys, 3000-6000 kN for titanium alloys, and 4000-8000 kN for nickel-based alloys. The rotation speed is controlled at 10-30 rpm, and the forging time is controlled at 1-5 minutes.
[0015] As a further technical solution of the present invention, the process monitoring includes using a thermocouple temperature sensor with an accuracy control of ±2°C, using a pressure sensor with an accuracy control of ±1% FS, using a speed sensor with an accuracy control of ±0.1rpm, and the sampling frequency of the data acquisition is 1 time per second. The automatic adjustment includes using a feedback control system to adjust the heating, pressure and speed in real time, and adjusting the fluctuation range according to the set process parameters.
[0016] As a further technical solution of the present invention, the annealing temperatures corresponding to the temperatures of the various alloys are 300-400°C for aluminum alloy, 600-700°C for titanium alloy, and 800-900°C for nickel-based alloys. The annealing times corresponding to the times of the various alloys are 1-2 hours for aluminum alloy, 2-4 hours for titanium alloy, and 2-4 hours for nickel-based alloys. The cooling methods corresponding to the cooling methods of the various alloys are air cooling for aluminum alloy, slow cooling in a furnace for titanium alloy, and slow cooling in a furnace for nickel-based alloys.
[0017] As a further technical solution of the present invention, the surface polishing is performed by mechanical polishing, the polishing particle size ranges from coarse to fine, and 80# to 1000# sandpaper is used for processing. The coating treatment includes spraying an anti-corrosion coating with a coating thickness controlled to be 20-50μm, and electroplating chrome or electroplating nickel with a coating thickness controlled to be 5-20μm.
[0018] As a further technical solution of the present invention, the nondestructive testing includes ultrasonic testing and X-ray testing, and the frequency of ultrasonic testing is 2-5MHz, the probe angle is 45°, the X-ray tube voltage is 150-300kV, and the testing frequency is controlled to test at least 1-2 pieces per batch of products, and each component in the key area is tested.
[0019] As a further technical solution of the present invention, the size and performance test includes size detection and performance test, the size detection adopts a laser rangefinder and a three-coordinate measuring machine, wherein the accuracy of the laser rangefinder is controlled to ±0.01mm, and the accuracy of the three-coordinate measuring machine is controlled to ±0.02mm, the performance test includes a tensile test and a hardness test, wherein the tensile test is in accordance with ASTM E8 standard, the loading rate of the testing machine is 0.5-2mm / min, and the hardness test adopts a Brinell hardness tester, and the test range is controlled to 10-300HB.
[0020] The beneficial effects of the present invention are as follows:
[0021] 1. The present invention significantly improves the quality and efficiency of alloy rod rotary forging by comprehensively optimizing the entire process from the design stage to inspection and quality control. In the material selection stage, the alloy composition and processing technology requirements are accurately matched to ensure that the mechanical properties, high temperature resistance and flow characteristics of the material meet high standards. Fine cleaning and heating during material pretreatment effectively remove surface impurities and preheat the material, laying a solid foundation for subsequent processing. Mold design optimization combined with finite element analysis ensures the rationality of the mold geometry and avoids drastic changes and folding risks in metal flow. High-precision temperature control and temperature uniformity control of the heating equipment, as well as precise parameter setting and online monitoring and adjustment during the forging process, further ensure the stability and consistency of the processing process. The refined operation of annealing and surface treatment not only improves the final performance of the product, but also enhances its corrosion resistance and aesthetics. Non-destructive testing and strict size and performance testing ensure that the product leaves the factory with zero defects, meeting customers' stringent requirements for high-quality alloy products. In summary, the method of the present invention effectively prevents folding defects, improves the overall quality and production efficiency of alloy rod rotary forging, and has significant technical and economic value.
[0022] 2. The present invention ensures the purity of the material surface and the uniformity of the internal structure through accurate material composition determination and efficient cleaning and heating process, laying a good material foundation for subsequent rotary forging processing. Secondly, the refinement of mold design and optimization, combined with finite element analysis technology, ensures the optimal working state of the mold during the processing process, and effectively avoids folding defects caused by unreasonable mold design. Precise parameter control and online monitoring adjustment during heating and forging further improve the stability and controllability of the processing process and reduce the impact of human operating errors on product quality. The meticulous operation of annealing and surface treatment not only eliminates the internal stress generated during the processing, but also improves the corrosion resistance and aesthetics of the product and extends the service life of the product. Finally, non-destructive testing and strict size and performance testing ensure comprehensive quality control of the product and meet the market demand for high-quality alloy products. In summary, the control method of the present invention not only solves the problem of folding defects in the rotary forging of alloy rods, but also improves the overall performance and production efficiency of the product through the optimization of the entire process, and has broad application prospects and promotion value. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the overall process of the present invention;
[0024] Figure 2 It is a schematic diagram of the process of the design stage of the present invention;
[0025] Figure 3 It is a schematic diagram of the process of the processing stage of the present invention;
[0026] Figure 4 It is a schematic diagram of the process of the post-processing stage of the present invention;
[0027] Figure 5 It is a schematic diagram of the process of inspection and quality control of the present invention. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] like Figures 1 to 5 As shown, in an embodiment of the present invention, a control method for avoiding folding defects during rotary forging of an alloy rod comprises the following steps:
[0030] S1: Design stage;
[0031] S2: processing stage;
[0032] S3 post-processing stage;
[0033] S4: Inspection and quality control;
[0034] The design stage includes material selection, material pretreatment, mold material selection, and mold design optimization. Material pretreatment includes material cleaning and material heating. Mold material selection includes finite element analysis, mold geometry design, and cooling channel design. The processing stage includes heating process, rotary forging process, online monitoring and adjustment. The heating process includes heating equipment, heating temperature, heating time, and temperature uniformity. The rotary forging process includes forging temperature, forging speed, pressure control, rotation speed, and forging time. Online monitoring and adjustment includes process monitoring, data acquisition, and automatic adjustment. The post-processing stage includes annealing and surface treatment. Annealing includes annealing temperature, annealing time, and cooling method. Surface treatment includes surface polishing and coating treatment. Inspection and quality control include non-destructive testing and size and performance testing.
[0035] By selecting the right material and cleaning and heating it during the design phase, the material, geometry and cooling channel design of the mold are optimized. The processing phase includes controlling the equipment, temperature, time and uniformity during the heating process, accurately adjusting the temperature, speed, pressure and time during the rotary forging process, and collecting data in real time and automatically adjusting the process through an online monitoring system. The post-processing phase includes appropriate annealing and surface treatment, such as annealing temperature, time and cooling method, as well as surface polishing and coating treatment. Finally, inspection and quality control are carried out through non-destructive testing and dimensional and performance testing to ensure that product quality meets standards, thereby effectively avoiding folding defects.
[0036] Preferably, material selection includes determining the specific composition of the alloy, and the alloy is preferably aluminum alloy, titanium alloy, and nickel-based alloy. The aluminum alloy adopts 7075 series, the titanium alloy adopts Ti-6Al-4V, and the nickel-based alloy adopts Inconel 718. It is necessary to select a suitable alloy according to the mechanical properties, high temperature resistance and flow characteristics of the material. When cleaning the material, a sulfuric acid-hydrofluoric acid mixed solution is used to clean the material for 5-10 minutes. After cleaning, deionized water is used to rinse the material for 3-5 minutes. Different heating parameters need to be set for different alloys for material heating, wherein the aluminum alloy needs to be heated to 450-500°C and maintained for 15-30 minutes, the titanium alloy needs to be heated to 800-900°C and maintained for 30-60 minutes, and the nickel-based alloy needs to be heated to 1100-1200°C and maintained for 30-60 minutes.
[0037] 7075 aluminum alloy, Ti-6Al-4V titanium alloy and Inconel 718 nickel-based alloy are used, and the materials are selected based on mechanical properties, high temperature resistance and flow characteristics to ensure high performance and applicability of the materials. After washing with a mixed solution of sulfuric acid and hydrofluoric acid and then rinsing with deionized water, impurities are effectively removed and the purity of the materials is improved. Heating parameters are set according to the characteristics of each alloy, and the heat treatment process is optimized, which not only enhances the material performance but also ensures the processing quality. This series of material selection and processing measures significantly improves the overall performance and reliability of the product.
[0038] Preferably, H13 steel and tungsten alloy are selected as mold materials. Finite element analysis includes using FEA software for simulation, analyzing alloy flow and stress distribution, adjusting mold design, ensuring uniform material flow, mold geometry including transition angle, not exceeding 10°, and avoiding sharp changes, and flow channel design adopts progressive contraction design, flow channel diameter: 20-30mm, width: 5-10mm, cooling channel design includes evenly distributing cooling channels in key areas of the mold, and controlling the channel diameter at 6-8mm.
[0039] H13 steel and tungsten alloy were selected as mold materials, and FEA software was used to accurately simulate alloy flow and stress distribution to optimize mold design. By ensuring uniform material flow, smooth transition of mold geometry, and progressive shrinkage flow channel design, the injection molding efficiency and product quality were significantly improved. At the same time, the evenly distributed cooling channel design effectively controls the temperature, ensuring stable operation and long life of the mold. This series of measures comprehensively improves mold performance and production efficiency.
[0040] Preferably, the heating equipment includes an induction heating resistance furnace, and the frequency is 100-200kHz, the power is 10-20kW, the temperature control accuracy is ±5°C, the heating temperature corresponds to the temperature of each alloy, aluminum alloy: 450-500°C, titanium alloy: 800-900°C, nickel-based alloy: 1100-1200°C, the heating time corresponds to the time of each alloy, aluminum alloy is controlled at 15-30 minutes, titanium alloy is controlled at 30-60 minutes, and nickel-based alloy is controlled at 30-60 minutes. The temperature uniformity includes using at least four temperature sensors to control the temperature fluctuation within ±10°C.
[0041] High-frequency induction heating resistance furnace is used to precisely control the frequency and power, and with high-precision temperature control technology, the optimal heating temperature and time are set for aluminum alloy, titanium alloy and nickel-based alloy to ensure the heat treatment effect of the alloy. Through the multi-point temperature sensing system, the uniformity of the heating temperature is effectively maintained, and the heating quality and efficiency are improved. This heating solution significantly optimizes the heat treatment process of alloy materials and ensures the consistency and stability of product performance.
[0042] Preferably, the forging temperature of each alloy is 400-500°C for aluminum alloy, 850-900°C for titanium alloy, and 1150-1200°C for nickel-based alloy. The forging speed corresponding to each alloy is 5-10mm / s for aluminum alloy, 2-5mm / s for titanium alloy, and 1-3mm / s for nickel-based alloy. The pressure control corresponding to each alloy is 2000-4000kN for aluminum alloy, 3000-6000kN for titanium alloy, and 4000-8000kN for nickel-based alloy. The rotation speed is controlled at 10-30rpm and the forging time is controlled at 1-5 minutes.
[0043] Precise forging temperatures and speeds are set for aluminum alloys, titanium alloys, and nickel-based alloys, combined with appropriate pressure control and rotation speed to ensure precise control of the forging process. This forging solution not only optimizes the microstructure of the alloy material, but also improves the mechanical properties and surface quality of the product. At the same time, by precisely controlling the forging time and pressure, efficient and stable forging production is achieved, improving overall production efficiency and product quality.
[0044] Preferably, process monitoring includes using a thermocouple temperature sensor with an accuracy control of ±2°C, using a pressure sensor with an accuracy control of ±1% FS, using a speed sensor with an accuracy control of ±0.1rpm, and the sampling frequency of data acquisition is 1 time per second. Automatic adjustment includes using a feedback control system to adjust heating, pressure and speed in real time, and adjusting the fluctuation range according to the set process parameters.
[0045] Through high-precision thermocouples, pressure and speed sensors, accurate monitoring of the forging process is achieved, ensuring strict control of temperature, pressure and speed. The data acquisition frequency of once per second ensures the timeliness of real-time monitoring, and the application of feedback control system can automatically adjust heating, pressure and speed to accurately control the fluctuation range of process parameters. This series of monitoring and adjustment measures has significantly improved the stability of the forging process and product quality, ensuring efficient and reliable production.
[0046] Preferably, the annealing temperatures corresponding to the temperatures of the various alloys are 300-400°C for aluminum alloys, 600-700°C for titanium alloys, and 800-900°C for nickel-based alloys. The annealing times corresponding to the times of the various alloys are 1-2 hours for aluminum alloys, 2-4 hours for titanium alloys, and 2-4 hours for nickel-based alloys. The cooling methods corresponding to the cooling methods of the various alloys are air cooling for aluminum alloys, slow cooling in a furnace for titanium alloys, and slow cooling in a furnace for nickel-based alloys.
[0047] Optimized annealing temperature and time are set for different alloys, combined with appropriate cooling methods, to effectively improve the microstructure and performance of alloy materials. Air cooling of aluminum alloys and slow furnace cooling of titanium alloys and nickel-based alloys ensure precise control of the annealing process. This annealing scheme improves the toughness, corrosion resistance and other comprehensive properties of the alloy, while enhancing the dimensional stability and service life of the product, providing a strong guarantee for the production of high-quality alloy products.
[0048] Preferably, the surface is polished by mechanical polishing with a polishing particle size ranging from coarse to fine using 80# to 1000# sandpaper, and the coating treatment includes spraying an anti-corrosion coating with a coating thickness controlled to be 20-50μm, and electroplating chrome or electroplating nickel with a coating thickness controlled to be 5-20μm.
[0049] Through the mechanical polishing process, sandpaper is used step by step from coarse to fine to ensure the surface finish and flatness of the alloy. Then, according to the needs, spray anti-corrosion coating or electroplating chrome / nickel is selected, and the coating thickness is strictly controlled, which not only enhances the corrosion resistance of the alloy, but also improves its appearance texture and wear resistance. This series of surface treatment measures significantly improves the comprehensive performance and service life of alloy products and meets the diverse application needs.
[0050] Preferably, nondestructive testing includes ultrasonic testing and X-ray testing, and the frequency of ultrasonic testing is 2-5MHz, the probe angle is 45°, the X-ray tube voltage is 150-300kV, and the testing frequency is controlled to test at least 1-2 pieces per batch of products, and each component in the key area is tested.
[0051] Ultrasonic and X-ray nondestructive testing technologies are used. Ultrasonic testing uses high frequency and specific probe angles to accurately locate internal defects, while X-rays penetrate materials through high voltage to clearly display the internal structure. We ensure that at least 1-2 pieces of each batch of products are tested, and conduct comprehensive testing of key areas, effectively ensuring the quality and safety of alloy products. The application of nondestructive testing technology has greatly improved the efficiency and accuracy of testing, providing a reliable means for continuous monitoring of product quality.
[0052] Preferably, the size and performance tests include size detection and performance testing. The size detection uses a laser rangefinder and a three-coordinate measuring machine, wherein the accuracy of the laser rangefinder is controlled to ±0.01mm, and the accuracy of the three-coordinate measuring machine is controlled to ±0.02mm. The performance test includes a tensile test and a hardness test, wherein the tensile test is in accordance with ASTM E8 standard, and the loading rate of the testing machine is 0.5-2mm / min. The hardness test uses a Brinell hardness tester, and the test range is controlled to 10-300HB.
[0053] High-precision laser rangefinders and three-coordinate measuring machines are used for dimensional inspection to ensure accurate measurement of alloy product dimensions. Performance evaluation combined with tensile testing and hardness testing follows international standards to ensure the authority and accuracy of test results. This series of rigorous dimensional and performance tests provides solid data support for quality control of alloy products, ensures the stability and reliability of product performance, and meets the strict requirements of customers.
[0054] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A control method for avoiding folding defects during rotary forging of alloy rods, characterized in that: The following steps are involved: S1: Design stage; S2: processing stage; S3 post-processing stage; S4: Inspection and quality control; The design stage includes material selection, material pretreatment, mold material selection, and mold design optimization. The material pretreatment includes material cleaning and material heating. The mold material selection includes finite element analysis, mold geometry design, and cooling channel design. The processing stage includes heating process, rotary forging process, online monitoring and adjustment. The heating process includes heating equipment, heating temperature, heating time, and temperature uniformity. The rotary forging process includes forging temperature, forging speed, pressure control, rotation speed, and forging time. The online monitoring and adjustment includes process monitoring, data acquisition, and automatic adjustment. The post-processing stage includes annealing and surface treatment. The annealing includes annealing temperature, annealing time, and cooling method. The surface treatment includes surface polishing and coating treatment. The inspection and quality control include non-destructive testing and size and performance testing.
2. A control method for avoiding folding defects during rotary forging of alloy rods according to claim 1, characterized in that: The material selection includes determining the specific composition of the alloy. The alloy is preferably aluminum alloy, titanium alloy, and nickel-based alloy. The aluminum alloy adopts the 7075 series, the titanium alloy adopts Ti-6Al-4V, and the nickel-based alloy adopts Inconel 718. The appropriate alloy needs to be selected according to the mechanical properties, high temperature resistance and flow characteristics of the material. When cleaning the material, a sulfuric acid-hydrofluoric acid mixed solution is used to clean the material for 5-10 minutes. After cleaning, deionized water is used to rinse the material for 3-5 minutes. The material heating needs to set different heating parameters according to different alloys, wherein the aluminum alloy needs to be heated to 450-500°C and maintained for 15-30 minutes, the titanium alloy needs to be heated to 800-900°C and maintained for 30-60 minutes, and the nickel-based alloy needs to be heated to 1100-1200°C and maintained for 30-60 minutes.
3. A control method for avoiding folding defects during rotary forging of alloy rods according to claim 1, characterized in that: The mold materials are H13 steel and tungsten alloy. The finite element analysis includes using FEA software for simulation, analyzing alloy flow and stress distribution, adjusting the mold design, and ensuring uniform material flow. The mold geometry includes a transition angle that does not exceed 10° and avoids sharp changes. The runner design adopts a progressive contraction design with a runner diameter of 20-30 mm and a width of 5-10 mm. The cooling channel design includes evenly distributing the cooling channels in key areas of the mold, and controlling the channel diameter to 6-8 mm.
4. A control method for avoiding folding defects during rotary forging of alloy rods according to claim 1, characterized in that: The heating equipment includes an induction heating resistance furnace, and the frequency is 100-200kHz, the power is 10-20kW, and the temperature control accuracy is ±5°C. The heating temperatures correspond to the temperatures of the various alloys: aluminum alloy: 450-500°C, titanium alloy: 800-900°C, and nickel-based alloy: 1100-1200°C. The heating time corresponds to the time of the various alloys: aluminum alloy is controlled at 15-30 minutes, titanium alloy is controlled at 30-60 minutes, and nickel-based alloy is controlled at 30-60 minutes. The temperature uniformity includes using at least four temperature sensors to control the temperature fluctuation within ±10°C.
5. A control method for avoiding folding defects during rotary forging of alloy rods according to claim 1, characterized in that: The forging temperatures of the various alloys are 400-500°C for aluminum alloy, 850-900°C for titanium alloy, and 1150-1200°C for nickel-based alloys. The forging speeds corresponding to the various alloys are 5-10mm / s for aluminum alloy, 2-5mm / s for titanium alloy, and 1-3mm / s for nickel-based alloys. The pressures controlled corresponding to the various alloys are 2000-4000kN for aluminum alloy, 3000-6000kN for titanium alloy, and 4000-8000kN for nickel-based alloys. The rotation speed is controlled at 10-30rpm, and the forging time is controlled at 1-5 minutes.
6. A control method for avoiding folding defects during rotary forging of alloy rods according to claim 1, characterized in that: The process monitoring includes using a thermocouple temperature sensor with an accuracy control of ±2°C, using a pressure sensor with an accuracy control of ±1% FS, using a speed sensor with an accuracy control of ±0.1rpm, the sampling frequency of the data acquisition is 1 time per second, and the automatic adjustment includes using a feedback control system to adjust the heating, pressure and speed in real time, and adjusting the fluctuation range according to the set process parameters.
7. A control method for avoiding folding defects during rotary forging of alloy rods according to claim 1, characterized in that: The annealing temperatures corresponding to the temperatures of the various alloys are 300-400°C for aluminum alloy, 600-700°C for titanium alloy, and 800-900°C for nickel-based alloy. The annealing times corresponding to the times of the various alloys are 1-2 hours for aluminum alloy, 2-4 hours for titanium alloy, and 2-4 hours for nickel-based alloy. The cooling methods corresponding to the cooling methods of the various alloys are air cooling for aluminum alloy, slow cooling in a furnace for titanium alloy, and slow cooling in a furnace for nickel-based alloy.
8. A control method for avoiding folding defects during rotary forging of alloy rods according to claim 1, characterized in that: The surface polishing is performed by mechanical polishing, and the polishing particle size ranges from coarse to fine, using 80# to 1000# sandpaper for processing. The coating treatment includes spraying an anti-corrosion coating with a coating thickness controlled to be 20-50μm, and electroplating chrome or electroplating nickel with a coating thickness controlled to be 5-20μm.
9. A control method for avoiding folding defects during rotary forging of alloy rods according to claim 1, characterized in that: The nondestructive testing includes ultrasonic testing and X-ray testing, and the frequency of ultrasonic testing is 2-5MHz, the probe angle is 45°, the X-ray tube voltage is 150-300kV, and the testing frequency is controlled to test at least 1-2 pieces per batch of products, and each component in the key area is tested.
10. A control method for avoiding folding defects during rotary forging of alloy rods according to claim 1, characterized in that: The size and performance tests include size detection and performance testing. The size detection uses a laser rangefinder and a three-coordinate measuring machine, wherein the accuracy of the laser rangefinder is controlled to ±0.01mm, and the accuracy of the three-coordinate measuring machine is controlled to ±0.02mm. The performance test includes a tensile test and a hardness test. The tensile test is in accordance with ASTM E8 standard, and the loading rate of the testing machine is 0.5-2mm / min. The hardness test uses a Brinell hardness tester, and the test range is controlled to 10-300HB.
Citation Information
Patent Citations
Method for determining mandrel rotary-forging axial feed process parameters of constant-speed universal transmission shaft
CN109158518A
Design method for inlet curved surface of rotary forging hammerhead die
CN113305253A
High-temperature forging control system for metal component and control system thereof
CN113634699A
Small-specification GH4141 high-temperature alloy bar and preparation method thereof