Preparation method of metal tea ware with microporous structure

The preparation method of metal teaware that forms a microporous structure by coating metal clay with support molds and sintering them to form a metal teaware, solves the problems of large weight and deformation of the silver teaware, and realizes the effect of lightening the teaware and improving water quality.

CN119057068AInactive Publication Date: 2024-12-03SHANGHAI CHENXI JEWELRY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411173245.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing preparation methods of metal tea utensils, the thickness of the silver tea utensils leads to large weight, high cost, and it is difficult to form hollow tea utensils and easily deformed. The prior art cannot effectively solve these problems.

Method used

The supporting mold is used to coat metal clay to form the embryo of the tea vessel. After natural moisture evaporation or low-temperature drying, it is compacted after sintering to form a microporous structure, reducing weight and increasing contact area.

Benefits of technology

The outer surface of the tea utensil is flat and sturdy, and a large number of microporous structures are formed on the middle and inner surfaces, which greatly reduces the overall weight, increases the metal contact area, improves the water quality and retains the fragrance effect. It is suitable for making teapots, tea cups and other utensils.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057068A_ABST
    Figure CN119057068A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a metal tea ware with a microporous structure, which comprises the following steps: S1) providing a support mold, and coating metal clay on the support mold to form a tea ware blank; s2) carrying out natural water evaporation or low-temperature drying to preliminarily shape the tea ware blank body; s3) sintering the preliminarily shaped tea ware blank, and melting and flowing out the supporting mold to form a metal tea ware; and S4) finally, compacting or shaping the metal tea ware. According to the preparation method of the metal tea ware with the micropore structure, the supporting mold is coated with the metal clay to form the tea ware blank, then the tea ware blank is shaped and sintered to form the metal tea ware, and finally surface pores are shrunk through pressure, so that the outer surface of the tea ware is flat and firm, and a large number of micropore structures are formed in the middle and the inner surface; the whole weight of the metal tea ware is greatly reduced, the metal contact area is increased, the water quality is improved, the fragrance is retained, and the metal tea ware is suitable for manufacturing teapots, teacups, tea cans, tea strainers and other utensils.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing metal tea utensils, in particular to a method for preparing metal tea utensils with a microporous structure. Background Art

[0002] Silver jewelry and its crafts are very popular. In the existing production process, silver jewelry is usually made by casting or forging. For silver tea sets, forging is used, and the wall thickness is generally between 0.4-0.7mm. Due to the thick wall thickness, the overall weight is large and the cost is high, which limits its promotion and application. In addition, the forging method requires the welding of joints, and residual additives and flux in the welds make the entire silver jewelry no longer 99% pure silver. Although the casting method can make the tea wall thinner, the custom casting mold is expensive, and the subsequent pattern often needs to be formed by engraving, which is more complicated.

[0003] In recent years, clay containing silver powder has been sold. The silver clay is molded into the shape that each person likes. After the molding is completed, it is placed in a cool place and sintered after drying. After completion, silver jewelry or silver arts and crafts jewelry with a predetermined shape is manufactured. For example, Chinese patent document CN1280045C discloses silver powder for silver clay and silver clay containing the silver powder; Chinese patent document CN101311138A discloses silver clay; and Chinese patent document CN101332507A discloses a silver clay and a method for making silver products using the silver clay.

[0004] However, the existing silver clay molding method is mainly for non-hollow, simple-shaped silver ornaments. For hollow tea sets, it is difficult to shape and easy to deform; the thinner the wall of the tea set, the more serious the deformation. Therefore, the existing preparation method of metal tea sets, especially silver tea sets, needs to be further improved. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing metal tea utensils with a microporous structure, which can ensure that the outer surface of the prepared tea utensils is smooth and firm, and a large number of microporous structures are formed in the middle and inner surfaces, which greatly reduces the overall weight of the metal tea utensils and increases the metal contact area, thereby achieving the effect of improving water quality and retaining fragrance.

[0006] The technical solution adopted by the present invention to solve the above technical problems is to provide a method for preparing metal tea utensils with a microporous structure, comprising the following steps: S1) providing a supporting mold, and coating metal clay on the supporting mold to form a tea utensil embryo; S2) subjecting the tea utensil embryo to a preliminary shape through natural water evaporation or low-temperature drying; S3) sintering the tea utensil embryo after the preliminary shape, and allowing the supporting mold to melt and flow out to form the metal tea utensil; S4) finally compacting or shaping the metal tea utensil.

[0007] Furthermore, the metal clay is gold clay, silver clay or copper clay, and the shrinkage rate of the metal clay is 5%-10%.

[0008] Furthermore, the metal clay is silver clay, the particle size of the silver powder is in the range of 0.5 μm-15 μm, and the proportions of the silver powders of various particle sizes are as follows:

[0009]

[0010] Furthermore, the step S1 also includes generating a bionic pattern or a personalized signature by pressing.

[0011] Furthermore, in step S1, the supporting mold is a wax mold with a softening temperature of 38°C-80°C; step S1 also includes controlling the temperature to 40°C-60°C, kneading and extruding the tea utensil embryo together with the supporting mold in a semi-softened state to generate a bionic pattern or a personalized signature.

[0012] Furthermore, in step S1, the supporting mold is a gypsum mold, and the melting temperature is 125°C-145°C.

[0013] Furthermore, the metal clay is silver clay, and the step S3 is to sinter the preliminarily shaped tea utensil embryo at a temperature of 500-680° C. to form the silver tea utensil.

[0014] Furthermore, in step S4, the outer surface and opening of the metal tea utensil are compacted to control the tap density to 2-10 g / mL, the scraping pressure to 1.0-5.0 tons, and the thickness of the metal tea utensil to 0.1-0.8 mm; for the wax mold, when the wall thickness of the metal tea utensil is less than 0.25 mm, a support frame is built inside the wax mold to prevent the wax from melting and flowing out, causing deformation of the tea utensil.

[0015] Furthermore, it also includes the later stage of grinding, polishing or coloring of the metal tea utensils.

[0016] Furthermore, when coloring, heating is used to wipe 2-5 times, and the heating temperature is controlled to be 80°C-120°C, so that the pigment diffuses along the microporous structure, and at the same time, the water evaporates to achieve a blurring and color fixing effect.

[0017] Compared with the prior art, the present invention has the following beneficial effects: the preparation method of metal tea utensils with a microporous structure provided by the present invention adopts a supporting mold to coat silver clay to form a tea utensil embryo, which is then shaped and sintered to form the metal tea utensil, and finally the surface pores are shrunk by pressure, so that the outer surface of the tea utensil is smooth and firm, and a large number of microporous structures are formed in the middle and inner surfaces, which greatly reduces the overall weight of the metal tea utensil and increases the metal contact area, thereby achieving the effect of improving water quality and retaining fragrance, and is suitable for making teapots, teacups, tea cans, tea strainers and other utensils. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a flow chart for preparing the teaware with a light and thin microporous structure of the present invention;

[0019] Figure 2 This is a structural diagram of a tea utensil embryo formed by coating silver clay on a supporting mold according to an embodiment of the present invention;

[0020] Figure 3 The structure diagram of the silver tea set after coloring prepared in the embodiment of the present invention;

[0021] Figure 4 This is a diagram of the internal microporous structure of the silver tea set made in an embodiment of the present invention. DETAILED DESCRIPTION

[0022] The present invention will be further described below in conjunction with the embodiments.

[0023] Figure 1 The present invention is a flow chart for preparing tea utensils with a thin and light microporous structure.

[0024] See also Figure 1 The present invention provides a method for preparing a metal tea utensil with a microporous structure, comprising the following steps:

[0025] S1) providing a supporting mold, coating the metal clay on the supporting mold to form a tea utensil embryo, such as Figure 2 As shown;

[0026] S2) the teaware embryo is initially shaped by natural water evaporation or low-temperature drying;

[0027] S3) sintering the preliminarily shaped tea utensil embryo, and allowing the supporting mold to melt and flow out to form a metal tea utensil;

[0028] S4) Finally, the metal tea set is compacted or reshaped; the pressure shrinks the surface pores, making the outer surface of the tea set smooth and firm, and forming a large number of microporous structures in the middle and inner surfaces, which greatly reduces the overall weight of the metal tea set; it has both good sealing properties and certain air permeability.

[0029] The metal clay used in the present invention can be gold clay, silver clay or copper clay, the shrinkage rate of the metal clay is 5%-10%, the crystal particle size is 0.1-30 μm, preferably 1-10 μm. Silver clay is preferably used, which not only greatly reduces the overall weight and cost of the silver tea set, but also has a microporous structure with a fragrance-retaining effect similar to that of a purple clay pot, and greatly increases the silver contact area, so as to better exert the sterilization and cooling effects of the silver metal.

[0030] The silver clay selected in the present invention can be the commonly used silver clay available on the market. As a preferred embodiment, it comprises the following components: silver powder, water-based adhesive, grease and water; the adhesive is a methylcellulose adhesive, which not only has good water solubility, but also makes it easier for the silver powder to form a microporous structure after sintering; the grease comprises glycerin and silicone oil, which can prevent stickiness and make the surface of the silver teaware have a certain shrinkage effect. The water-based adhesive can be cellulose, carrageenan or an organic resin, preferably a methylcellulose adhesive or an ethyl cellulose adhesive, so that the silver clay has better ductility. As a preferred embodiment, the mass fraction of each component is as follows:

[0031]

[0032] The particle size of silver powder is 0.1 micron to 30 microns. In order to form a more uniform microporous structure, the particle size of silver powder ranges from 0.5μm to 15μm. The proportions of silver powder of different particle sizes are as follows:

[0033]

[0034] The method for preparing a metal tea set with a microporous structure provided by the present invention, said step S1 further comprises generating a bionic pattern by pressing, such as leaving the texture of insects, leaves, specimens or fingerprints, to make a bionic pot, and the fingerprint can be used as a personalized signature. Preferably, the supporting mold in said step S1 is a wax mold, such as Figure 3 As shown. The softening temperature of the wax mold is 38°C-80°C; the step S1 also includes controlling the temperature to 40°C-60°C, and kneading and squeezing the tea utensil embryo together with the supporting mold in a semi-softened state to make various special-shaped pots. If the softening or melting temperature of the supporting mold is too low, and it melts before the metal clay is solidified and fixed, the product will be deformed by its own weight or the weight of the supporting mold. Especially for wax molds, when the wall thickness of the metal tea utensil is less than 0.25mm, it is necessary to build a shelf inside the wax mold to support it to prevent the deformation of the tea utensil when the wax melts and flows out.

[0035] As another preferred embodiment, in step S1, the supporting mold is a plaster mold, and the melting temperature is 125°C-145°C.

[0036] In order to better form a microporous structure, the sintering temperature can be reduced as much as possible. After repeated tests, for copper powder, the sintering temperature is preferably 600°C-750°C, and the sintering time is 35 minutes-60 minutes; for gold powder, the sintering temperature is preferably 750 degrees-950°C, and the sintering time is 10 minutes-60 minutes. For silver powder, it needs to be sintered at a temperature greater than 450 degrees and lower than 910 degrees; preferably, for silver clay, the step S3 sinters the preliminarily shaped tea utensil embryo at a temperature of 500-680°C to form a silver tea utensil, and the sintering time is 10 minutes-30 minutes.

[0037] In order to ensure that the outer surface of the tea set is flat and firm and has good sealing performance, step S4 of the present invention compacts the outer surface and opening of the metal tea set, controls the tap density to 2-10g / mL, controls the scraping pressure to 1.0-5.0 tons, and controls the thickness of the metal tea set to be as thin as 0.1-0.8mm.

[0038] The preparation method of the metal tea set with microporous structure provided by the present invention also includes grinding, polishing or coloring the metal tea set in the later stage. When coloring, the metal tea set is heated and wiped 2-5 times, and the heating temperature is controlled to be 80℃-120℃. The pigment is prevented from accumulating by multiple wiping, so that the pigment diffuses along the microporous structure. At the same time, the heating control is used to make the water evaporate quickly to achieve the effect of blurring and fixing the color; ensuring that the metal tea set will not have mottled and discolored problems due to a long time, such as Figure 3 shown.

[0039] The method for preparing a metal tea set with a microporous structure provided by the present invention comprises the following steps: coating a supporting mold with silver clay to form a tea set embryo, then shaping and sintering the metal tea set, and finally shrinking the surface pores by pressure, so that the outer surface of the tea set is smooth and firm, and a large number of microporous structures are formed in the middle and inner surfaces, such as Figure 4 As shown. In this way, the contact area of ​​the metal is greatly increased, and it is suitable for making teapots, teacups, tea cans, tea strainers and other utensils. Taking the silver teapot as an example, the silver teapot made by the present invention is similar to the purple clay teapot, which not only achieves the effect of improving water quality and retaining fragrance; but also reduces the weight by more than 70% compared with the existing silver teapot, greatly reducing the overall weight and cost of the silver tea set.

[0040] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art may make some modifications and improvements without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the definition of the claims.

Claims

1. A method for preparing a metal tea set with a microporous structure, It is characterized in that The steps include: S1) providing a supporting mold, and applying metal clay on the supporting mold to form a tea utensil embryo; S2) the teaware embryo is initially shaped by natural water evaporation or low-temperature drying; S3) sintering the preliminarily shaped tea utensil embryo, and allowing the supporting mold to melt and flow out to form a metal tea utensil; S4) finally compacting or shaping the metal tea set.

2. The method for preparing the metal tea utensil with microporous structure as claimed in claim 1, It is characterized in that The metal clay is gold clay, silver clay or copper clay, and the shrinkage rate of the metal clay is 5%-10%.

3. The method for preparing the metal tea utensil with microporous structure as claimed in claim 2, It is characterized in that The metal clay is silver clay, the particle size of the silver powder is in the range of 0.5 μm-15 μm, and the proportions of the silver powders of different particle sizes are as follows:

4. The method for preparing the metal tea utensil with microporous structure as claimed in claim 1, It is characterized in that The step S1 also includes generating a bionic pattern or a personalized signature by pressing.

5. The method for preparing the metal tea utensil with microporous structure as claimed in claim 4, It is characterized in that In step S1, the supporting mold is a wax mold with a softening temperature of 38°C-80°C; step S1 also includes controlling the temperature to 40°C-60°C, kneading and squeezing the tea utensil embryo together with the supporting mold in a semi-softened state to generate a bionic pattern or a personalized signature.

6. The method for preparing the metal tea utensil with microporous structure as claimed in claim 1, It is characterized in that In step S1, the supporting mold is a gypsum mold, and the melting temperature is 125° C.-145° C.

7. The method for preparing the metal tea utensil with microporous structure as claimed in claim 1, It is characterized in that The metal clay is silver clay, and the step S3 is to sinter the preliminarily shaped tea utensil embryo at a temperature of 500-680° C. to form the silver tea utensil.

8. The method for preparing the metal tea utensil with microporous structure as claimed in claim 1, It is characterized in that The step S4 compacts the outer surface and opening of the metal tea set, controls the tap density to 2-10 g / mL, controls the scraping pressure to 1.0-5.0 tons, and controls the thickness of the metal tea set to 0.1-0.8 mm; for the wax mold, when the wall thickness of the metal tea set is less than 0.25 mm, a support is built in the wax mold to prevent the wax from melting and flowing out, causing deformation of the tea set.

9. The method for preparing the metal tea utensil with microporous structure as claimed in claim 1, It is characterized in that It also includes the later stage of grinding, polishing or coloring of metal tea utensils.

10. The method for preparing the metal tea utensil with microporous structure as claimed in claim 9, It is characterized in that When coloring, use heating method to wipe 2-5 times, control the heating temperature to 80℃-120℃, so that the pigment diffuses along the microporous structure, and at the same time the water evaporates to achieve the effect of blurring and fixing the color.

Citation Information

Patent Citations

  • TiAl alloy powder near-net-shaping method

    CN103586468A

  • Method of manufacturing metal parts having geometric structures such as thin wall or thin groove

    CN103878372A

  • Metal clay and molding sintering method based on flexible metallic paper

    CN110814334A

  • Production of ornament having the same surface state as ornament produced with noble metal clay

    JP1999033675A

  • Method for making fragnant porous metal sintering body

    KR1020040013342A