Silver-based active brazing filler metal for medium-temperature hard alloy and preparation method of silver-based active brazing filler metal

The combination of silver-based active brazing material is prepared by combining high-energy ball milling of silver-copper-titanium alloy powder and organic binder, which solves the problems of easy oxidation of active brazing material and unstable welding quality, and realizes high-strength connection of medium-temperature cemented carbide and Low thermal stress, suitable for a variety of welding processes.

CN119057305APending Publication Date: 2024-12-03CHINA RAILWAY 18TH BUREAU GRP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411249320.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing active solder is easily oxidized during welding, resulting in unstable welding quality, difficult to meet the high strength and low thermal stress requirements of cemented carbide, and insufficient flexibility in welding process.

Method used

Silver-copper-titanium alloy powder is used to form silver-copper-titanium active brazing through high-energy ball milling, and paste-shaped brazing is prepared by adding organic binder, and block silver-based active brazing is prepared by discharge plasma sintering, which increases the chemical stability of welding and mechanical properties.

Benefits of technology

The preparation of silver-based active brazing material for medium-temperature cemented carbide has good wetting properties, low melting temperature and excellent mechanical properties, reducing thermal stress and thermal damage to the substrate during welding process, and is suitable for a variety of Brazing process, flexible process operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057305A_ABST
    Figure CN119057305A_ABST
Patent Text Reader

Abstract

The invention discloses silver-based active brazing filler metal for medium-temperature hard alloy and a preparation method of the silver-based active brazing filler metal. The silver-based active brazing filler metal for the medium-temperature hard alloy is composed of, by mass, 3-8% of titanium and the balance silver-copper alloy powder, and further, the silver-based active brazing filler metal for the medium-temperature hard alloy can further comprise, by mass, 0.5-6% of reinforced phase particles. The prepared silver-based active brazing filler metal for the medium-temperature hard alloy has the low working temperature, so that the influence of thermal stress on a base material is reduced, and the risks of deformation and heat loss are reduced. And in addition, good mechanical performance is achieved at the medium-high temperature, and high-strength reliable connection can be formed. The prepared silver-based active brazing filler metal for the medium-temperature hard alloy has good wettability on most of alloys, is further suitable for connection of various different materials, and is high in adaptability and wide in application range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of welding materials, and more specifically to a silver-based active solder for medium-temperature hard alloy and a preparation method thereof. Background Art

[0002] Active solder refers to a solder formed by adding reactive components to conventional solder. The added active components are elements such as titanium, zirconium, hafnium, niobium, etc., which can react with substances with electronic coordination stability. These elements will undergo a series of reactions with the base material to form an interface reaction layer combined with the metal, which can achieve infiltration and welding of the base material. However, active solder has active characteristics and is easily oxidized in the atmosphere. When it is oxidized, it loses its function as an active solder and cannot undergo effective chemical reactions with the base material. Therefore, it must be effectively protected before application and during use. Before welding, the solder is placed at the oven mouth or in a vacuum bag. Usually, welding is performed in a vacuum or highly pure protective gas environment. The vacuum degree during welding should be as high as possible. Among the active solders currently used, titanium is the most commonly used active ingredient. The active ingredient commonly used in solder is titanium. The following are common active solders containing titanium: Ag-Cu-Ti, Cu-Zn-Ti, Ti-Zr-Ni-Cu, Sn-Ag-Ti, Ni-Pd-Ti, Pd-Au-Ni-Ti, etc. Among these materials, the research on Ag-Cu-Ti solder is the earliest, and this series of solders has good wettability for most alloy materials.

[0003] In order to meet the use requirements of cemented carbide and obtain a brazed joint with strength stability and reliability. The brazing material is required to have good fluidity and good wetting of the base material. It should also have the advantages of good plasticity, toughness and high strength. At the same time, the melting point of the brazing material is required to be within the specified range. Generally, the brazing material composition is selected from eutectic alloy composition alloys. Eutectic composition alloys have the advantages of low melting point and good fluidity, which is conducive to the brazing material wetting the base material and filling the gap to form a good joint. In addition, in order to prevent the formation of brittle phases between the brazing material and the base material and reduce the connection strength of the joint, the brazing material and the base material are required to generate a solid solution structure with good plasticity as much as possible.

[0004] According to the melting point of the solder, active solder can be roughly divided into three types: low-temperature active solder, medium-temperature active solder and high-temperature active solder.

[0005] (1) Low-temperature active solder: Active solder based on tin or lead, with a melting point below 300°C. It has little demand on the base material and does not require any treatment before welding. It does not require the use of flux or shielding gas during the welding process.

[0006] (2) Medium-temperature active solder: a reactive solder mainly containing silver. The melting point of silver-based active solder is about 800°C. It has good processing and mechanical properties, as well as excellent thermal conductivity, electrical conductivity and corrosion resistance. It is currently the most widely studied and effective active solder in the world.

[0007] (3) High-temperature active brazing filler metals: mainly active brazing filler metals based on high-temperature or precious metals such as Pt, Ni, Pd, Co, and Au. The brazing joints can work at a high temperature of about 800°C.

[0008] When designing active brazing filler metal connectors, the following aspects should be noted:

[0009] (1) The solder must have an appropriate melting temperature. Usually, its initial crystallization temperature is 40-50°C lower than the solidus of the base material.

[0010] (2) During welding, the brazing material has a good wetting effect and can effectively fill the gaps in the weld;

[0011] (3) Ensure a close connection between the two through physical and chemical interaction with the parent material;

[0012] (4) The solder cannot contain chemical components with high saturated vapor pressure such as Cd and Mg;

[0013] (5) The solder should have good plasticity, low yield strength and high tensile strength to ensure low residual stress at room temperature;

[0014] (6) The welding materials have good creep resistance, thermal fatigue and corrosion resistance, ensuring that the welded joints can be used under harsh working conditions. Summary of the invention

[0015] In order to overcome the deficiencies and shortcomings of the prior art, the primary purpose of the present invention is to provide a method for preparing a silver-based active solder for medium-temperature hard alloy. The preparation method first adds two alloy powders, silver-copper alloy powder and titanium powder, for high-energy ball milling to form a silver-copper-titanium active solder, then adds an appropriate amount of organic binder to prepare a paste solder, and then obtains a block of silver-based active solder for medium-temperature hard alloy by spark plasma sintering. Furthermore, reinforcing phase particles (molybdenum, boron or yttrium oxide) can be added to the two alloy powders to mix into a silver-copper-titanium composite active solder powder. The preparation method is highly flexible and relatively simple for studying the mechanism of action of various alloy elements on silver-based solder. The composition ratio of each element can be freely controlled to control the changes in the microstructure and crystal structure of the solder alloy. It is simple and easy to analyze the formation of the brazing seam, the microstructure in the brazing seam, the distribution of brittle phases and the mechanical properties of the brazed joint.

[0016] Although paste solder is widely used in various fields due to its advantages such as easy application, reduced waste, improved welding quality and adaptability to complex shapes, block solder is easy to handle and store, and can accurately control the dosage and consistency and uniformity of the composition, which makes block solder a more popular choice in many industrial applications.

[0017] Another object of the present invention is to provide a silver-based active solder for medium-temperature cemented carbide prepared by the above method, which has a very low melting temperature and excellent mechanical properties, and can reduce the thermal stress and thermal damage to the substrate during the brazing process. At the same time, the silver-based active solder is suitable for a variety of brazing processes, has flexible process operations, and exhibits good chemical stability in many working environments.

[0018] The primary purpose of the present invention is achieved through the following technical solutions:

[0019] A method for preparing a silver-based active solder for medium-temperature cemented carbide comprises the following steps:

[0020] (1) Preparation of silver-copper-titanium solder alloy powder / silver-copper-titanium solder composite alloy powder: all alloy powders are mixed and high-energy ball milled, dried, and sieved to obtain silver-copper-titanium solder alloy powder / silver-copper-titanium solder composite alloy powder;

[0021] (2) Preparation of paste solder: silver-copper-titanium solder alloy powder / silver-copper-titanium solder composite alloy powder and an organic binder are mixed, stirred, and sealed to obtain a paste solder;

[0022] (3) Preparation of bulk solder: solidifying and sintering the paste solder in step (2) by spark plasma sintering to obtain bulk solder, i.e., silver-based active solder for medium-temperature cemented carbide;

[0023] All the alloy powders in step (1) are silver-copper alloy powder, titanium powder or silver-copper alloy powder, titanium powder and reinforcing phase particles; the reinforcing phase particles are at least one of molybdenum, boron or yttrium oxide;

[0024] The organic binder in step (2) comprises the following components in volume percentage: 30-40 vol.%, 30-40 vol.% of ethylene glycol methyl ether, and the balance of ethyl acetate;

[0025] Wherein, the main solvent in the organic binder is ethylene glycol methyl ether and ethylene glycol ethyl ether, and the auxiliary solvent is ethyl acetate.

[0026] Preferably, when the alloy powder in step (1) is silver-copper alloy powder or titanium powder, the silver-copper-titanium solder alloy powder has the following mass percentage components: 3-8% titanium powder and the balance silver-copper alloy powder.

[0027] Preferably, the silver-copper-titanium solder alloy powder in step (1) is composed of the following components by mass fraction: 92% silver-copper alloy powder and 8% titanium powder.

[0028] Preferably, when the alloy powder in step (1) is silver-copper alloy powder, titanium powder and reinforcing phase particles, the silver-copper-titanium solder alloy powder is composed of the following components in percentage by mass: 3-8% titanium powder, 0.5-6% reinforcing phase particles, and the remainder is silver-copper alloy powder.

[0029] Preferably, the silver-copper-titanium solder alloy powder in step (1) is composed of the following components in mass fraction: 88.32% silver-copper alloy powder, 7.68% titanium powder and 4% molybdenum powder.

[0030] Preferably, the silver-copper-titanium solder alloy powder in step (1) is composed of the following components in mass fraction: 91.45% silver-copper alloy powder, 7.95% titanium powder and 0.4% boron powder.

[0031] Preferably, the silver-copper-titanium solder alloy powder in step (1) is composed of the following components in mass fraction: 91.44% silver-copper alloy powder, 7.96% titanium powder and 0.5% molybdenum powder.

[0032] Among them, the silver-copper alloy powder mentioned above is spherical with a particle size of 48 μm, the particle size of the titanium powder is 20 μm, the particle size of the boron powder is 200 nm, the particle size of the molybdenum powder is 1 μm, and the particle size of the yttrium oxide powder is 500 nm.

[0033] Preferably, in step (1), the ball milling speed is 200-300 rpm; the ball-to-material ratio is 8:1; three types of grinding balls with diameters of 10 mm, 6 mm, and 3 mm are used to mix the silver-copper-titanium solder alloy powder, and the ball milling atmosphere is argon; the ball milling time is 12-24 h.

[0034] Preferably, the drying temperature in step (1) is 50 to 80° C. and the drying time is 2 to 6 hours.

[0035] Preferably, in step (2), the weight ratio of the silver-copper-titanium solder alloy powder to the organic binder is 9:1, and mechanical stirring is used to fully mix the powder, the stirring speed is 120 r / min, and the stirring time is 15 to 30 minutes.

[0036] Preferably, the sealed storage in step (2) is to pour the paste solder into a syringe, seal it, and store it at 0°C.

[0037] Preferably, in step (3), the sintering atmosphere is vacuum, the heating rate is 60-100° C. / min, the sintering temperature is 800-900° C., the holding time is 10-20 min, and the pressure is 20-50 MPa.

[0038] Another object of the present invention is achieved by the following technical solutions:

[0039] A silver-based active solder for medium-temperature hard alloy is prepared by the above preparation method.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] (1) The silver-based active solder for medium-temperature cemented carbide prepared by the present invention has good wettability to most alloys and is also suitable for connecting a variety of different materials, has strong adaptability and a wide range of applications;

[0042] (2) The silver-based active solder for medium-temperature cemented carbide prepared by the present invention has a lower working temperature, which helps to reduce the impact of thermal stress on the substrate and reduce the risk of deformation and heat loss. It also has good mechanical properties at medium and high temperatures and can form a high-strength reliable connection;

[0043] (3) The preparation method of the silver-based active solder for medium-temperature cemented carbide provided by the present invention is highly flexible, and is relatively simple for studying the mechanism of action of various alloy elements on the silver-based solder. The composition ratio of each element can be freely controlled to control the changes in the microstructure and crystal structure of the solder alloy, and is simple and easy to analyze the formation of the solder joint, the microstructure in the solder joint, the distribution of the brittle phase, and the mechanical properties of the brazed joint;

[0044] (4) The silver-based active solder for medium-temperature cemented carbide prepared by the present invention has a wetting angle of 15.2-20.7° on the surface of YG15 cemented carbide and a wetting angle of 7.3-13.5° on the surface of 42CrMo steel. According to differential scanning calorimetry, the solidus temperature TS of the obtained solder powder is 783°C and the liquidus temperature TL is 811°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly explain the technical aspects of the embodiments of the present invention, the accompanying drawings in the specification of the embodiments will be briefly described below.

[0046] Figure 1 The DSC graph of the silver-based active solder for medium-temperature cemented carbide prepared in Example 1;

[0047] Figure 2 The wetting angle of the silver-based active solder for medium-temperature cemented carbide prepared in Example 3 on the YG15 surface;

[0048] Figure 3 This is the wetting angle of the silver-based active solder for medium-temperature cemented carbide prepared in Example 3 on the 42CrMo surface. DETAILED DESCRIPTION

[0049] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0050] Example 1

[0051] A method for preparing a silver-based active solder for medium-temperature cemented carbide comprises the following steps:

[0052] (1) Weigh 47g of silver-copper alloy powder (48μm, purity 99.9%) and 3g of titanium powder (20μm, purity 99.9%) in a glove box. Place the two weighed metal powders in a ball mill and evacuate to 1MPa. Then introduce argon gas and use a QM-2SP20-CL planetary ball mill for ball milling. The ball milling speed is 300r / min, the ball milling time is 24h, the ball-to-material ratio is 8:1, and the diameters of the stainless steel grinding balls are 10mm, 6mm, and 3mm. Place the mixed powder in a vacuum drying oven to remove moisture at 80℃ for 8h to obtain silver-copper-titanium solder alloy powder.

[0053] (2) For the preparation of paste solder, an organic binder needs to be prepared. Prepare an organic binder with a volume ratio of 40 vol.% of ethylene glycol methyl ether, 40 vol.% of ethylene glycol ethyl ether, and 20 vol.% of ethyl acetate in a test tube. The specific content of each component of the organic binder will be optimized secondary according to the actual viscosity, volatility, and organizational conditions. Mix the organic binder with the silver-copper-titanium solder alloy powder, and the weight ratio of the silver-copper-titanium solder alloy powder to the organic binder is 9:1; use mechanical stirring to fully mix, the stirring speed is 120r / min, and the stirring time is 20 minutes. Test whether the viscosity of each point in the paste filler is consistent. Stop stirring when it meets the standard, and fill the gelatinous intermediate layer into a syringe, seal it, and store it at 0°C;

[0054] (3) For bulk solder, spark plasma sintering is used to solidify the powder. The obtained silver-copper-titanium alloy powder is filled into a graphite mold and then spark plasma sintered. The temperature is raised to 800°C at a rate of 100°C / min and kept at this temperature for 10 minutes, and the pressure is set to 30MPa. After the insulation is completed, the furnace is cooled to obtain a bulk silver-copper-titanium alloy solder, that is, a silver-based active solder for medium-temperature cemented carbide.

[0055] The silver-based active brazing filler metal for medium-temperature cemented carbide described in this embodiment has a wetting angle of 15.2° on the surface of YG15 cemented carbide and a wetting angle of 7.3° on the surface of 42CrMo steel. According to the differential scanning calorimetry test, the solidus temperature TS of the obtained silver-based active brazing filler metal for medium-temperature cemented carbide is 783°C, the liquidus temperature TL is 811°C, and the melting temperature is 783°C. The average shear strength of brazing YG15 cemented carbide and 42CrMo steel with the silver-based active brazing filler metal for medium-temperature cemented carbide is 231MPa.

[0056] Example 2

[0057] A method for preparing a silver-based active solder for medium-temperature cemented carbide comprises the following steps:

[0058] (1) Considering the density difference of each component in the composite solder, 45.12g of silver-copper alloy powder (48μm, purity 99.9%) and 2g of molybdenum powder (1μm, purity 99.9%) were weighed in a glove box. The two weighed metal powders were placed in a ball mill and evacuated to 1MPa, and then argon was introduced and ball milled with a QM-2SP20-CL planetary ball mill. The ball milling speed was 300r / min, the ball milling time was 12h, the ball-to-material ratio was 8:1, and the diameters of the stainless steel grinding balls were 10mm, 6mm, and 3mm; 2.88g of titanium powder (20μm, purity 99.9%) was added to the mixed powder and the ball milling was continued for 12h; finally, the silver-copper-titanium-molybdenum composite solder powder obtained by ball milling was placed in a vacuum drying oven to remove moisture at 80℃ for 8h to obtain a silver-copper-titanium-molybdenum composite solder alloy powder.

[0059] (2) For the paste silver-copper-titanium-molybdenum composite solder, an organic binder needs to be prepared. Prepare an organic binder with a volume ratio of 40 vol.% of ethylene glycol methyl ether and 40 vol.% of ethylene glycol ethyl ether and 20 vol.% of ethyl acetate in a test tube. The specific content of each component of the organic binder will be optimized secondary according to the actual viscosity, volatility, and organization. Mix the organic binder with the silver-copper-titanium-molybdenum composite solder alloy powder, and the weight ratio of the silver-copper-titanium-molybdenum composite solder alloy powder to the organic binder is 9:1. Use mechanical stirring to mix thoroughly, the stirring speed is 120r / min, the stirring time is 20 minutes, test whether the viscosity of each point in the paste filler is consistent, stop stirring after reaching the standard, fill the gelatinous intermediate layer into the syringe, seal it, and store it at 0°C.

[0060] (3) For bulk silver-copper-titanium-molybdenum composite brazing filler metal, the powder is solidified by spark plasma sintering. The obtained silver-copper-titanium-molybdenum alloy powder is filled into a graphite mold and then spark plasma sintered. The temperature is raised to 800°C at a rate of 100°C / min and kept at this temperature for 10 minutes, and the pressure is set to 30MPa. After the insulation is completed, the furnace is cooled to obtain a bulk silver-copper-titanium-molybdenum active brazing filler metal, i.e., a silver-based active brazing filler metal for medium-temperature cemented carbide.

[0061] The wetting angle of the silver-based active brazing filler metal for medium-temperature cemented carbide described in this embodiment on the surface of YG15 cemented carbide is 19.4°, and the wetting angle on the surface of 42CrMo steel is 12.1°; according to the differential scanning calorimetry test, the solidus temperature TS of the obtained silver-based active brazing filler metal for medium-temperature cemented carbide is 783°C, the liquidus temperature TL is 810°C, and the melting temperature is 796°C. The average shear strength of brazing YG15 cemented carbide and 42CrMo steel with the silver-based active brazing filler metal for medium-temperature cemented carbide is 245MPa.

[0062] Example 3

[0063] A method for preparing a silver-based active solder for medium-temperature cemented carbide comprises the following steps:

[0064] (1) Considering the density difference of each component in the composite solder, 0.5g boron powder (200nm, purity 99.9%) and 2.97g titanium powder (20μm, purity 99.9%) were weighed in a glove box. The two weighed metal powders were placed in a ball mill and evacuated to 1MPa, and then argon was introduced and ball milled with a QM-2SP20-CL planetary ball mill. The ball milling speed was 300r / min, the ball milling time was 12h, the ball-to-material ratio was 8:1, and the diameters of the stainless steel grinding balls were 10mm, 6mm, and 3mm; 46.53g silver-copper alloy powder (48μm, purity 99.9%) was added to the mixed powder and the ball milling was continued for 12h; finally, the silver-copper-titanium-boron composite solder powder obtained by ball milling was placed in a vacuum drying oven to remove moisture at 80℃ for 8h to obtain a silver-copper-titanium-boron composite solder alloy powder.

[0065] (2) For paste-like silver-copper-titanium-boron composite solder, an organic binder needs to be prepared. Prepare an organic binder with a volume ratio of 40 vol.% of ethylene glycol methyl ether and 40 vol.% of ethylene glycol ethyl ether and 20 vol.% of ethyl acetate in a test tube. The specific content of each component of the organic binder will be optimized secondary according to the actual viscosity, volatility, and organization. Mix the organic binder with the silver-copper-titanium-boron solder alloy powder, and the weight ratio of the silver-copper-titanium-boron solder alloy powder to the organic binder is 9:1. Use mechanical stirring to mix thoroughly, the stirring speed is 120r / min, the stirring time is 20 minutes, test whether the viscosity of each point in the paste filler is consistent, stop stirring after reaching the standard, fill the gelatinous intermediate layer into the syringe, seal it, and store it at 0°C.

[0066] (3) For bulk silver-copper-titanium-boron composite brazing filler metal, the powder is solidified by spark plasma sintering. The obtained silver-copper-titanium-boron alloy powder is filled into a graphite mold and then spark plasma sintered. The temperature is raised to 800°C at a rate of 100°C / min and kept at this temperature for 10 minutes, and the pressure is set to 30MPa. After the insulation is completed, the furnace is cooled to obtain a bulk silver-copper-titanium-boron active brazing filler metal, i.e., a silver-based active brazing filler metal for medium-temperature cemented carbide.

[0067] The silver-based active brazing filler metal for medium-temperature cemented carbide described in this embodiment has a wetting angle of 21.7° on the surface of YG15 cemented carbide and a wetting angle of 13.5° on the surface of 42CrMo steel. According to the differential scanning calorimetry test, the solidus temperature TS of the obtained silver-based active brazing filler metal for medium-temperature cemented carbide is 783°C, the liquidus temperature TL is 810°C, and the melting temperature is 790°C. The average shear strength of brazing YG15 cemented carbide and 42CrMo steel with the silver-based active brazing filler metal for medium-temperature cemented carbide is 251MPa.

[0068] Example 4

[0069] A method for preparing a silver-based active solder for medium-temperature cemented carbide comprises the following steps:

[0070] (1) Considering the density difference of each component in the composite solder, 0.25g yttrium oxide powder (500nm, purity 99.9%) and 2.985g titanium powder (20μm, purity 99.9%) were weighed in a glove box. The two weighed metal powders were placed in a ball mill and evacuated to 1MPa, and then argon was introduced and ball milled with a QM-2SP20-CL planetary ball mill. The ball milling speed was 300r / min, the ball milling time was 12h, the ball-to-material ratio was 8:1, and the diameters of the stainless steel grinding balls were 10mm, 6mm, and 3mm; 46.765g silver-copper alloy powder (48μm, purity 99.9%) was added to the mixed powder and continued to ball mill for 12h; finally, the silver-copper-titanium-yttrium oxide composite solder powder obtained by ball milling was placed in a vacuum drying oven to remove moisture at 80℃ for 8h to obtain silver-copper-titanium-yttrium oxide composite solder alloy powder.

[0071] (2) For the paste-like silver-copper-titanium-yttrium oxide composite solder, an organic binder needs to be prepared. Prepare an organic binder with a volume ratio of 40 vol.% of ethylene glycol methyl ether, 40 vol.% of ethylene glycol ethyl ether, and 20 vol.% of ethyl acetate in a test tube. The specific content of each component of the binder will be optimized secondary according to the actual viscosity, volatility, and organization. Mix the organic binder with the silver-copper-titanium-yttrium oxide composite alloy powder, and the weight ratio of the silver-copper-titanium-yttrium oxide solder alloy powder to the organic binder is 9:1. Use mechanical stirring to mix thoroughly, the stirring speed is 120r / min, the stirring time is 20 minutes, test whether the viscosity of each point in the paste filler is consistent, stop stirring after reaching the standard, fill the gelatinous intermediate layer into the syringe, seal it, and store it at 0°C.

[0072] (3) For bulk silver-copper-titanium-yttrium oxide active brazing filler metal, the powder is solidified by spark plasma sintering. The obtained silver-copper-titanium-yttrium oxide active powder is filled into a graphite mold and then spark plasma sintered. The temperature is raised to 800°C at a heating rate of 100°C / min and kept at this temperature for 10 minutes, and the pressure is set to 30MPa. After the insulation is completed, the furnace is cooled to obtain a bulk silver-copper-titanium-yttrium oxide active brazing filler metal, i.e., a silver-based active brazing filler metal for medium-temperature cemented carbide.

[0073] The silver-based active brazing filler metal for medium-temperature cemented carbide described in this embodiment has a wetting angle of 15.9° on the surface of YG15 cemented carbide and a wetting angle of 8.7° on the surface of 42CrMo steel. According to the differential scanning calorimetry test, the solidus temperature TS of the obtained silver-based active brazing filler metal for medium-temperature cemented carbide is 783°C, the liquidus temperature TL is 811°C, and the melting temperature is 783°C. The average shear strength of brazing YG15 cemented carbide and 42CrMo steel with the silver-based active brazing filler metal for medium-temperature cemented carbide is 259MPa.

[0074] By comparing Examples 1 to 4 and existing alloy solders, it can be seen that the silver-based active solder for medium-temperature cemented carbide of the present invention has good wettability with the base material, a lower melting point and a narrower melting range, and can ensure high-strength connection between medium-temperature cemented carbide and steel. The low melting point can effectively reduce the oxidation and brittle phase generation during welding, and has a smaller melting zone, which is more conducive to metallurgical reactions during welding.

[0075]

[0076] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a silver-based active solder for medium-temperature cemented carbide, characterized in that: The following steps are included: (1) Preparation of silver-copper-titanium solder alloy powder / silver-copper-titanium solder composite alloy powder: all alloy powders are mixed and high-energy ball milled, dried, and sieved to obtain silver-copper-titanium solder alloy powder / silver-copper-titanium solder composite alloy powder; (2) Preparation of paste solder: silver-copper-titanium solder alloy powder / silver-copper-titanium solder composite alloy powder and an organic binder are mixed, stirred, and sealed to obtain a paste solder; (3) Preparation of bulk solder: solidifying and sintering the paste solder in step (2) by spark plasma sintering to obtain bulk solder, i.e., silver-based active solder for medium-temperature cemented carbide; All the alloy powders in step (1) are silver-copper alloy powder, titanium powder or silver-copper alloy powder, titanium powder and reinforcing phase particles; the reinforcing phase particles are at least one of molybdenum, boron or yttrium oxide; The organic binder in step (2) comprises the following components in volume percentage: 30-40 vol.%, 30-40 vol.% of ethylene glycol methyl ether, and the balance of ethyl acetate; Wherein, the main solvent in the organic binder is ethylene glycol methyl ether and ethylene glycol ethyl ether, and the auxiliary solvent is ethyl acetate.

2. The method for preparing the silver-based active solder for medium-temperature cemented carbide according to claim 1, characterized in that: When the alloy powder in step (1) is silver-copper alloy powder or titanium powder, the silver-copper-titanium solder alloy powder is composed of the following components in percentage by mass: 3-8% titanium powder and the remainder silver-copper alloy powder.

3. The method for preparing the silver-based active solder for medium-temperature cemented carbide according to claim 2, characterized in that: The silver-copper-titanium solder alloy powder in step (1) is composed of the following components by mass fraction: 92% silver-copper alloy powder and 8% titanium powder.

4. The method for preparing the silver-based active solder for medium-temperature cemented carbide according to claim 1, characterized in that: When the alloy powder in step (1) is silver-copper alloy powder, titanium powder and reinforcing phase particles, the silver-copper-titanium solder alloy powder is composed of the following components in percentage by mass: 3-8% titanium powder, 0.5-6% reinforcing phase particles, and the remainder is silver-copper alloy powder.

5. The method for preparing the silver-based active solder for medium-temperature cemented carbide according to claim 1, characterized in that: In step (1), the ball milling speed is 200-300 rpm; the ball-to-material ratio is 8:1; three kinds of grinding balls with diameters of 10 mm, 6 mm and 3 mm are used to mix the silver-copper-titanium solder alloy powder, and the ball milling atmosphere is argon; the ball milling time is 12-24 hours.

6. The method for preparing the silver-based active solder for medium-temperature cemented carbide according to claim 1, characterized in that: The drying temperature in step (1) is 50 to 80° C. and the drying time is 2 to 6 hours.

7. The method for preparing the silver-based active solder for medium-temperature cemented carbide according to claim 1, characterized in that: In step (2), the weight ratio of the silver-copper-titanium solder alloy powder to the organic binder is 9:1, and mechanical stirring is used to fully mix the powder, the stirring speed is 120 r / min, and the stirring time is 15 to 30 minutes.

8. The method for preparing the silver-based active solder for medium-temperature cemented carbide according to claim 1, characterized in that: The sealed storage in step (2) is to fill the paste solder into a syringe, seal it, and store it at 0°C.

9. The method for preparing the silver-based active solder for medium-temperature cemented carbide according to claim 1, characterized in that: In step (3), the sintering atmosphere is vacuum, the heating rate is 60-100°C / min, the sintering temperature is 800-900°C, the holding time is 10-20min, and the pressure is 20-50MPa.

10. A silver-based active solder for medium-temperature cemented carbide, characterized in that: Prepared according to any one of the preparation methods of claims 1 to 9.