Method for preparing high-silicon hierarchical pore molecular sieve by using low-silicon molecular sieve
High silicon multi-stage porous molecular sieve was prepared by reacting low-silicon molecular sieve with acidic solution and combining the inorganic alkali, salt and silicon source, which solved the problems of complex operation, high cost and environmental pollution in the prior art, and achieved high efficiency, Preparation of environmentally friendly high-silicon multi-stage pore molecular sieve.
Patent Information
- Application Number
- CN202411005323.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-12-03
AI Technical Summary
The existing multi-stage pore molecular sieve preparation methods are complicated in operation and harsh in reaction conditions, and it is impossible to synthesize high-silicon molecular sieve, which is costly and inefficient, and relies on organic template agents to pollute the environment.
Low-silicon molecular sieve mixed with acidic solution and heated to dealuminize, then added inorganic alkali, salt, silicon source and water to form mother liquor, and re-crystallized to prepare high-silicon multi-stage porous molecular sieve without template agents, and regulate the growth of molecular sieve The environment improves the silicon-aluminum ratio.
The low-cost and environmentally friendly high-silicon multi-stage porous molecular sieve preparation is achieved, which improves the crystallinity and mesoporous polymorphism of molecules, and the molecular sieve has good stability, avoiding harmful gas release and structural damage.
Smart Images

Figure CN119059529A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of molecular sieve synthesis, and specifically relates to a method for preparing a multi-level pore molecular sieve with high crystallinity, many mesopores and increased silicon-aluminum ratio by first dealumination and then recrystallization. Background Art
[0002] Zeolite is an inorganic crystalline aluminosilicate with uniformly distributed molecular-scale pores. It is widely used in industry in the fields of adsorption, separation and catalysis. Molecular sieves with pore sizes between 0.3 and 2 nm are generally called microporous molecular sieves. They have good selectivity and provide special activity for catalytic reactions. However, microporous molecular sieves also have some disadvantages, such as the pore length is too long, resulting in large diffusion resistance of molecules, reducing the rate and selectivity of catalytic reactions; the pore diameter is too small, which limits the entry of larger molecules and reduces the utilization rate and scope of application of molecular sieves.
[0003] In recent years, multi-level pore molecular sieves have attracted widespread attention. Multi-level pore molecular sieves refer to molecular sieve materials with both micropores and mesopores (2-50nm) or micropores and macropores (>50nm) in the molecular sieve crystals. Multi-level pore molecular sieves can combine the good selectivity of micropores with the high specific surface area, high catalytic activity and high diffusion performance of mesopores or macropores, thereby improving the catalytic efficiency and stability of molecular sieves. There are mainly the following methods for preparing multi-level pore molecular sieves.
[0004] Steam treatment method, under high temperature conditions, treats the molecular sieve with water vapor to hydrolyze the molecular sieve framework, remove the aluminum atoms in the framework, form defects and amorphous phases, and then generate mesopores or macropores. The amorphous phase formed after treatment can be removed by acid leaching. This method is mainly used for Y-type molecular sieves, which can increase the specific surface area and pore volume of the molecular sieve, but it will also cause partial deactivation and structural damage of the molecular sieve.
[0005] Acid-base treatment method, soaking the molecular sieve in an acidic or alkaline solution, dissolving the aluminum or silicon in the molecular sieve framework to form mesopores or macropores. This method is mainly used for Y-type molecular sieves, X-type molecular sieves, β molecular sieves and ZSM-5, etc., which can increase the surface area and mesopore volume of the molecular sieve, but it will also change the acidity and stability of the molecular sieve.
[0006] Chemical treatment method uses some special chemical reagents such as SiCl4, EDTA, (NH4)2SiF6, etc. to react with molecular sieves to remove aluminum or silicon in the molecular sieve framework and form mesopores or macropores. This method can prepare multi-level pore molecular sieves without changing the molecular sieve crystal form, but the reaction conditions are harsh.
[0007] The template method uses an organic or inorganic template to react with a silicon source and an aluminum source under hydrothermal conditions to generate a molecular sieve with an ordered or disordered mesoporous structure. In the subsequent calcination process, the template is burned away, leaving mesopores or macropores. This method can prepare various types of multi-level pore molecular sieves, but it cannot hydrothermally synthesize high-silicon FAU. Most of them are used to synthesize molecular sieves with high silicon-aluminum ratios, such as ZSM-5, ZSM-12, and MCM-22. The cost of the template is high, and high-temperature calcination or acid leaching is required to remove the template, resulting in energy consumption and environmental pollution.
[0008] Precursor assembly method: This method uses the precursor of microporous molecular sieve, such as aluminosilicate or molecular sieve, as a seed, and assembles with a template or other inorganic species to form a partially or completely crystallized pore wall, thereby improving the hydrothermal stability and acidity of the molecular sieve. The advantage of this method is that it can synthesize multi-level porous molecular sieves with high stability, such as MPS-9, MSU-U, etc., but the disadvantage is that it requires a higher amount of template and water, and the synthesis process is more complicated.
[0009] CN111375441A discloses a method for preparing a multi-level pore HZSM-5 molecular sieve, wherein the raw powder of the ZSM-5 molecular sieve is first calcined and then mixed with a mixed alkaline solution of an inorganic base and an organic base, wherein the organic base is selected from at least one of tetrapropylammonium hydroxide (TPAOH) and tetrabutylammonium hydroxide (TBAOH), then mixed with an acid solution, ion exchanged with an ammonium salt solution, and finally dried and calcined to obtain. The prepared molecular sieve has a regular MFI skeleton structure, while retaining a large number of microporous structures, a certain amount of non-penetrating mesoporous structure is introduced, so that it combines the advantages of microporous ZSM-5 molecular sieve and mesoporous material, and the macromolecules produced in the biomass catalytic thermal cracking process can easily enter and stay in the active site of the molecular sieve, shorten the diffusion path, reduce the diffusion resistance of the reactant molecules and the product molecules in the pores, and increase the probability of the reactant molecules contacting the active site, thereby increasing the aromatic carbon yield and reducing the coke generation.
[0010] CN110937609A discloses a method for preparing a multi-level pore FAU structure molecular sieve, wherein a FAU structure molecular sieve precursor is subjected to steam treatment and alkali treatment, and the treated product is roasted. The multi-level pore FAU structure molecular sieve has high crystal shape retention, a wide range of silicon-aluminum ratio applications, uniform micropore and mesopore distribution, good acidity, and can be converted into a hydrogen type or other ionic type multi-level pore FAU structure molecular sieve by ion exchange.
[0011] CN109422283A discloses a method for preparing a molecular sieve with a multi-level pore structure. The molecular sieve uses a molecular sieve with crystal defects as a seed to undergo hydrothermal crystallization treatment, thereby obtaining a molecular sieve with a multi-level pore structure. No expensive mesoporous template is required in the synthesis process, which can effectively save costs and effectively limit the loss of discarded molecular sieves with crystal defects that occur during the synthesis process.
[0012] The current methods for synthesizing hierarchical pore molecular sieves all have certain defects, such as possible adverse effects on the skeleton structure and performance of the molecular sieves, cumbersome operation steps, low efficiency, dependence on organic solvents and templates, and burden on energy and the environment. Therefore, it is urgently needed to develop a simple, efficient and environmentally friendly method for synthesizing hierarchical pore molecular sieves. Summary of the invention
[0013] The purpose of the present invention is to solve the problems of the existing multi-level pore molecular sieve preparation method, such as cumbersome operation steps, harsh reaction conditions, inability to synthesize high-silicon molecular sieves, high cost, low efficiency, dependence on organic templates, and environmental pollution. The present invention develops a method with low cost, simple operation process, and no use of organic templates, and a method for making a microporous low-silicon molecular sieve into a multi-level pore molecular sieve with high crystallinity, many mesopores, and increased silicon-aluminum ratio. The present invention dissolves part of the framework aluminum through acid treatment to obtain a modified molecular sieve, and then adjusts the growth environment of the molecular sieve by adding soluble sodium salts and alkali to obtain a multi-level pore molecular sieve with an increased silicon-aluminum ratio. Compared with other alkali metal salts or alkaline earth metal salts, the spatial size and charge characteristics of sodium metal ions are more conducive to the formation of high-silicon multi-level pore molecular sieves.
[0014] One aspect of the present invention provides a method for preparing a high-silicon multi-level pore molecular sieve using a low-silicon molecular sieve, comprising the following steps:
[0015] (1) mixing a low-silicon molecular sieve with an acidic solution, and carrying out a dealumination reaction under heating and stirring conditions. After the reaction is completed, the mixture is subjected to solid-liquid separation, washing, and drying to obtain a modified high-silicon molecular sieve;
[0016] (2) Inorganic alkali, salt, silicon source, aluminum source and water are mixed and stirred to form a mother liquor, and then the modified high-silicon molecular sieve prepared in step (1) is added thereto, mixed evenly and then re-crystallized, and then filtered and washed to obtain a multi-level pore molecular sieve product with an increased silicon-aluminum ratio, and no template is used in the crystallization process.
[0017] The low-silicon molecular sieve described in step (1) is one of low-silicon molecular sieves such as FAU, FER, MOR, CHA, LTA, and LTL.
[0018] The low-silicon molecular sieve specifically refers to a molecular sieve with a framework Si / Al≤4, preferably a molecular sieve with Si / Al≤3.5, and more preferably a molecular sieve with Si / Al≤3.
[0019] The acidic solution described in step (1) is an organic acid and / or an inorganic acid, the inorganic acid is one or more of sulfuric acid, hydrochloric acid, phosphoric acid, and ammonium fluorosilicate, and the organic acid is one or more of EDTA, oxalic acid, and citric acid; the mother liquor in step (1) is a gel or a sol.
[0020] During the acid treatment, the concentration of the acid solution is 0.01-12 mol / L, preferably 0.1-5 mol / L; the mass ratio of the molecular sieve to the acid solution is 1-100, preferably 5-20.
[0021] The acid treatment temperature in step (1) is 20-120°C for 0.1-96h; preferably, the treatment temperature is 50-80°C for 1-12h.
[0022] The acid treatment in step (1) can be carried out under normal pressure or in a pressurized container.
[0023] The ratio of the aluminum source, silicon source, alkali, salt and water in step (2) is prepared according to a molar ratio of 0-0.1:1-10:0.1-1:0.3-0.8:10-100, wherein the aluminum source is calculated as aluminum oxide and the silicon source is calculated as silicon dioxide; preferably, the ratio of the aluminum source, silicon source, alkali, salt and water is prepared according to a molar ratio of 0.01-0.06:3-8:0.3-0.7:0.4-0.6:30-70.
[0024] The alkali described in step (2) is one or more of NaOH, KOH, Ca(OH)2, Sr(OH)2; the silicon source is one or more of common silicon sources such as sodium silicate, TEOS, silica sol, fumed silica, macroporous silica gel, etc.
[0025] The salt described in step (2) is a soluble sodium salt, more preferably one or more of sodium sulfate, sodium nitrate, sodium chloride and sodium fluoride.
[0026] In step (2), the recrystallization conditions are 20-150° C. for 1-48 hours; preferably, the recrystallization conditions are 50-120° C. for 5-24 hours.
[0027] The mass ratio of the mother liquor to the molecular sieve in step (2) is 1 to 20, preferably 3 to 10.
[0028] The recrystallization reaction described in step (2) is carried out in a closed reaction vessel with or without pressure.
[0029] Another aspect of the present invention discloses a high-silicon multi-level pore Y-type molecular sieve prepared by the above method, wherein the high-silicon mesoporous Y-type molecular sieve is highly crystallized and has intracrystalline mesopores, wherein the mesopore volume of the multi-level pore molecular sieve can reach more than 0.20mL / g, and retains more than 95% of the micropore volume of the original molecular sieve, and the micropore volume is retained from more than 0.35mL / g of the original molecular sieve to more than 0.33mL / g; the framework silicon-to-aluminum ratio of the high-silicon mesoporous Y-type molecular sieve is ≥4, more preferably ≥5, and compared with the original molecular sieve, the framework silicon-to-aluminum ratio is increased by more than 20%, more preferably by more than 25%; preferably, the silicon-to-aluminum ratio is increased by less than 80%, more preferably by less than 50%, and most preferably by 30-41%.
[0030] Compared with the prior art, the method provided by the present invention for preparing a multi-level pore molecular sieve with high crystallinity, many mesopores, and increased silicon-aluminum ratio using a low-silicon molecular sieve has at least the following advantages: no organic template is used, the cost is low, and the preparation process is green and environmentally friendly; roasting is used to avoid the release of harmful gases and the damage to the zeolite structure; a multi-level pore molecular sieve with increased silicon-aluminum ratio is obtained by a hydrothermal synthesis method, and the molecular sieve has good stability. Compared with the comparative example, although the silicon-aluminum ratio of the molecular sieve finally obtained in the comparative example is higher than that of the molecular sieve finally obtained in the present invention, it can be found from the XRD spectrum of comparative example 1 that the crystallinity of the molecular sieve finally obtained is extremely low, and the degree of increase of the mesopores of the molecular sieve finally obtained in comparative examples 2 and 3 is not as high as that of the present invention, and its preparation process is more complicated. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The XRD spectra of the industrial NaY molecular sieve of Example 1 of the present invention and the acid-treated ET-72;
[0032] Figure 2 This is a scanning electron microscope image of the industrial NaY molecular sieve of Example 1 of the present invention;
[0033] Figure 3 This is a scanning electron microscope image of ET-72 after acid treatment in Example 1 of the present invention;
[0034] Figure 4 XRD spectra of ET-72-T90 and ET-72-T100 molecular sieves obtained at different crystallization temperatures in Examples 1-3 of the present invention;
[0035] Figure 5 This is a scanning electron microscope image of the ET-72-T90 molecular sieve obtained in Example 1 of the present invention;
[0036] Figure 6 This is a transmission electron microscope image of the ET-72-T90 molecular sieve obtained in Example 1 of the present invention;
[0037] Figure 7 This is a scanning electron microscope image of the ET-72-T100 molecular sieve obtained in Example 2 of the present invention;
[0038] Figure 8 The nitrogen adsorption-desorption isotherms of the industrial NaY molecular sieves, the acid-treated ET-72, and the obtained ET-72-T90 and ET-72-T100 molecular sieves of Examples 1-3 of the present invention;
[0039] Fig. 9 The evaluation results of industrial NaY molecular sieve, ET-72-T90 and ET-72-T100 molecular sieves of Example 4 of the present invention as catalysts for the dealkylation reaction of 1,3,5-triisopropylbenzene (TiPBz) are shown;
[0040] Fig.10 XRD spectra of the industrial NaY molecular sieve of Comparative Example 1 of the present invention, the CS-Y after acid treatment, and the obtained CS-Y-T90 molecular sieve;
[0041] Fig.11 This is a scanning electron microscope image of the industrial NaY molecular sieve of Comparative Example 1 of the present invention;
[0042] Fig.12 This is a scanning electron microscope image of CS-Y after acid treatment in Comparative Example 1 of the present invention;
[0043] Fig.13 This is a scanning electron microscope image of the CS-Y-T90 molecular sieve obtained in Comparative Example 1 of the present invention;
[0044] Fig.14 The nitrogen adsorption-desorption isotherms of the industrial NaY molecular sieve of Comparative Example 1 of the present invention, the CS-Y after acid treatment, and the obtained CS-Y-T90 molecular sieve; DETAILED DESCRIPTION
[0045] The following examples are used to further illustrate the present invention, but are not intended to limit the present invention.
[0046] Example 1
[0047] Add 300g of deionized water to the PP bottle, then add 9.64g of EDTA to it, and stir vigorously at 800rpm in an oil bath at 100℃ until it dissolves. Weigh 20g of NaY molecular sieve (sample name NaY) with a SAR of 2.6, add it to the solution, and stir vigorously for 72h. After stirring, put the product into a centrifuge for centrifugal washing, and after sufficient washing, put it into a 65℃ oven to dry to obtain a high-silicon powdered molecular sieve with defect sites (sample name ET-72). Weigh 20g of mother liquor and 2g of ET-72 respectively and move them into the PP bottle and stir for 60min. Then move it into a 50ml polytetrafluoroethylene-lined stainless steel pressure-resistant reactor, and then place the sealed reactor in a 90℃ oven for crystallization for 24 hours. After the crystallization is completed, the mixture is centrifuged and washed, and after sufficient washing, it is placed in a 100℃ oven to dry to obtain a high-silicon mesoporous Y-type molecular sieve (sample name is ET-72-T90). The XRD pattern, scanning electron microscopy, transmission electron microscopy, nitrogen adsorption-desorption isotherms and pore structure data of the sample are shown in Figure 4 , Figure 5 , Figure 6 , Figure 8 And as shown in Table 1.
[0048] Example 2
[0049] Add 300g of deionized water to the PP bottle, then add 9.64g of EDTA to it, and stir vigorously at 800rpm in an oil bath at 100℃ until it dissolves. Weigh 20g of NaY molecular sieve (sample name NaY) with a SAR of 2.6, add it to the solution, and stir vigorously for 72h. After stirring, put the product into a centrifuge for centrifugal washing, and after sufficient washing, put it into a 65℃ oven to dry to obtain a high-silicon powdered molecular sieve with defect sites (sample name ET-72). Weigh 20g of mother liquor and 2g of ET-72 respectively and move them into the PP bottle and stir for 60min. Then move it into a 50ml polytetrafluoroethylene-lined stainless steel pressure-resistant reactor, and then place the sealed reactor in a 100℃ oven for crystallization for 24 hours. After the crystallization is completed, the mixture is centrifuged and washed, and after sufficient washing, it is placed in a 100℃ oven to dry to obtain a high-silicon mesoporous Y-type molecular sieve (sample name is ET-72-T100). The XRD pattern, SEM image, nitrogen adsorption-desorption isotherm and pore structure data of the sample are shown in Figure 4 , Figure 7 , Figure 8 And as shown in Table 1.
[0050] Example 3
[0051] Add 300g of deionized water to the PP bottle, then add 9.64g of EDTA to it, and stir vigorously in an oil bath at 100℃ at 800rpm until it dissolves. Weigh 20g of NaY molecular sieve (sample name NaY) with a SAR of 2.6, add it to the solution, and stir vigorously for 72h. After stirring, put the product into a centrifuge for centrifugal washing, and after sufficient washing, put it into a 65℃ oven to dry to obtain a high-silicon powdered molecular sieve with defect sites (sample name ET-72). Weigh 20g of mother liquor and 2gET-72 respectively and move them into the PP bottle and stir for 60min. Then move it into a 50ml polytetrafluoroethylene-lined stainless steel pressure-resistant reactor, and then place the sealed reactor in a 120℃ oven for crystallization for 24 hours. After the crystallization is completed, the mixture is centrifuged and washed, and after sufficient washing, it is placed in a 100℃ oven to dry to obtain a high-silicon mesoporous Y-type molecular sieve (sample name is ET-72-T120).
[0052] Table 1
[0053]
[0054] S BET a is the specific surface area determined by isothermal adsorption method; S ext b is the external specific surface area; V micro b is the micropore volume; V meso c is the mesopore volume.
[0055] Example 4
[0056] The original NaY molecular sieve, the ET-72-T90 molecular sieve obtained in Example 1, and the ET-72-T100 molecular sieve obtained in Example 2 were used as catalysts for the dealkylation reaction of 1,3,5-triisopropylbenzene (TiPBz). Each experiment was carried out at atmospheric pressure (1×10 5 Pa) into a reactor (5 mm in diameter, 1300 mm in length) and enclosed between two layers of inert SiC (size range 200-400 μm). The sample was heated in a dry air flow (50 mL min -1 ) was activated at 100 °C for 1 h and then heated to 450 °C (at a heating rate of 1.5 °C min -1 ) and maintained at this temperature for 3 hours. Then N2 was introduced to cool the reactor to a reaction temperature of 350°C. 100 mL·min -1 The N2 gas flow enters a saturator filled with TiPBz and the temperature is maintained at 71℃ (P TiPBz=180Pa). The unique space-time W / F0 used is 380kg·s·mol -1 Stable conditions were established in less than 5 minutes. The first product was collected after 5 minutes and then every 15 minutes. The quantitative analysis was performed on a CPG (VARIAN Cp 3800; HP-Pona 50m, 0.2mm, 0.5μm column) equipped with a FID detector. The evaluation results were as follows: Fig. 9 As shown. It can be seen that the Y molecular sieve with multi-level pores containing micropores, mesopores and macropores can be used in the dealkylation reaction of 1,3,5-triisopropylbenzene, which can significantly improve its conversion rate and the catalyst has good stability.
[0057] Comparative Example 1
[0058] Add 250g of deionized water to the PP bottle, then add 25g of ammonium sulfate, and stir vigorously at 500rpm at room temperature until it dissolves. Weigh 25g of NaY molecular sieve with a SAR of 2.6 (sample name NaY), add it to the solution and stir evenly. Add 87.5g of 1mol / L oxalic acid solution to the solution and stir for 2h. After stirring, place the product in a centrifuge for centrifugal washing, and after sufficient washing, place it in a 100℃ oven to dry to obtain a high-silicon powdered molecular sieve with defect sites (sample name CS-Y). Weigh 20g of the mother liquor and 2g of CS-Y respectively and move them into the PP bottle and stir for 60min. Then transfer it into a 50ml polytetrafluoroethylene lined stainless steel pressure reactor, and then place the sealed reactor in a 100°C oven for crystallization for 24 hours. After the crystallization is completed, the mixture is centrifuged and washed, and after sufficient washing, it is placed in a 100°C oven to dry to obtain a high-silicon mesoporous Y-type molecular sieve (sample name is CS-Y-T90). The XRD pattern, scanning electron microscope image, nitrogen adsorption and desorption isotherm and pore structure data of the sample are shown in Figure 1. Fig.10 , Fig.11 , Fig.12 , Fig.13 , Fig.14 And as shown in Table 2.
[0059] Table 2
[0060]
[0061] S BET a is the specific surface area determined by isothermal adsorption method; S ext b is the external specific surface area; V micro b is the micropore volume; V meso c is the mesopore volume.
[0062] Comparative Example 2
[0063] Heat 1000mL of 0.75mol / L NaOH aqueous solution to 95°C. Then, add 100g of NaY molecular sieve (sample name NaY) to the heated solution. Place the product in a centrifuge for centrifugal washing, and after sufficient washing, place it in a 100°C oven to dry to obtain sample ATY. Use 1.5mol / L NH4Cl solution, with a solution to molecular sieve ratio of 10mL / g, and perform ion exchange on NaY and ATY three times at 90°C to prepare NH4 + Type samples. NH4-ATY and NH4-NaY zeolites were aged in 100% steam at 650°C for 2 hours. The aged samples were treated again with 1.5 mol / L NH4Cl solution at 95°C for 1 hour, and the pH of the NH4Cl solution was adjusted to 2.5-2.6 with hydrochloric acid (1 mol / L). After the exchange, the mixture was centrifuged and washed, and after sufficient washing, it was placed in a 100°C oven and dried to obtain the final product. The ultra-stable Y-type molecular sieve prepared from the parent NaY is named USY, and the final product prepared from the ATY molecular sieve is named ATUSY. The pore structure data and silicon-aluminum ratio of this group of samples are shown in Table 3.
[0064] Table 3
[0065]
[0066] S BET a is the specific surface area determined by isothermal adsorption method; S ext b is the external specific surface area; V micro b is the micropore volume; V meso c is the mesopore volume.
[0067] Comparative Example 3
[0068] Weigh 100g NH4Cl and 1000g H2O and add them to a PP bottle and mix them evenly. Add 100g NaY and stir them evenly at room temperature. Add 100mL of 1mol / L oxalic acid to the PP bottle and stir for 30min, then raise the temperature to 90℃ and stir for 1h. Put the product into a centrifuge for centrifugal washing, and after sufficient washing, put it in a 100℃ oven to dry to obtain the sample OTY. Stir 10g NaY and OTY molecular sieves with 10g ammonium chloride and 100g water respectively, and then raise the temperature to 90℃ and stir for 1h. For OTY molecular sieves, the same NH4 exchange is repeated 3 times. After the exchange is completed, the mixture is centrifuged and washed and dried in a 100℃ oven. The ammonium-exchanged NaY and OTY molecular sieves are aged in 100% steam at 650℃ for 2 hours. 10g of the aged sample was mixed evenly with 10g of ammonium chloride and 100g of water respectively, the solution was heated to 95℃ and stirred for 1h, and the pH of the NH4Cl solution was adjusted to 3.05 (for NaY) or 2.5 (for OTY) with hydrochloric acid (1mol / L). After the exchange, the mixture was centrifuged and washed, and after sufficient washing, it was placed in a 100℃ oven to dry to obtain the final product. The ultra-stable Y-type molecular sieve prepared from the parent NaY is named USY, and the final product prepared from the OTY molecular sieve is named OTUSY. The pore structure data and silicon-aluminum ratio of this group of samples are shown in Table 4.
[0069] Table 4
[0070]
[0071] S BET a is the specific surface area determined by isothermal adsorption method; S ext b is the external specific surface area; V micro b is the micropore volume; V meso c is the mesopore volume.
[0072] The above embodiments describe the basic principles and main features of the present invention and the advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention, and are not intended to limit the scope of the present invention in any way. Without departing from the scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the protection required.
Claims
1. A method for preparing a high-silicon multi-level pore molecular sieve using a low-silicon molecular sieve, comprising the following steps: (1) mixing a low-silicon molecular sieve with an acidic solution, and carrying out a dealumination reaction under heating and stirring conditions. After the reaction is completed, the mixture is subjected to solid-liquid separation, washing, and drying to obtain a modified high-silicon molecular sieve; (2) Inorganic alkali, salt, silicon source, aluminum source and water are mixed and stirred to form a mother liquor, and then the modified high-silicon molecular sieve prepared in step (1) is added thereto, mixed evenly and then re-crystallized, and then filtered and washed to obtain a multi-level pore molecular sieve product with an increased silicon-aluminum ratio, and no template is used in the crystallization process.
2. The method according to claim 1, characterized in that The low-silicon molecular sieve described in step (1) is one of low-silicon molecules such as FAU, FER, MOR, CHA, LTA, and LTL.
3. The method according to claim 1, characterized in that The low-silicon molecular sieve specifically refers to a molecular sieve with a framework Si / Al≤4, preferably a molecular sieve with Si / Al≤3.5, and more preferably a molecular sieve with Si / Al≤3.
4. The method according to claim 1, characterized in that The acidic solution in step (1) is an organic acid and / or an inorganic acid, the inorganic acid is one or more of sulfuric acid, hydrochloric acid, phosphoric acid, and ammonium fluorosilicate, and the organic acid is one or more of EDTA, oxalic acid, and citric acid; the mother liquor in step (1) is a gel or a sol; And / or, in step (1), the concentration of the acidic solution is 0.01-12 mol / L, preferably 0.1-5 mol / L; the mass ratio of the molecular sieve to the acidic solution is 1-100, preferably 5-20; And / or, the acid treatment temperature in step (1) is 20-120°C for 0.1-96h; preferably, the treatment temperature is 50-80°C for 1-12h; And / or, the acid treatment in step (1) can be carried out under normal pressure or in a pressurized container.
5. The method according to claim 1, characterized in that The ratio of the aluminum source, silicon source, alkali, salt and water in step (2) is prepared according to a molar ratio of 0-0.1:1-10:0.1-1:0.3-0.8:10-100, wherein the aluminum source is calculated as aluminum oxide and the silicon source is calculated as silicon dioxide; preferably, the ratio of the aluminum source, silicon source, alkali, salt and water is: The preparation is carried out in a molar ratio of 0.01~0.06:3~8:0.3~0.7:0.4~0.6:30~70.
6. The method according to claim 1, characterized in that The alkali in step (2) is one or more of NaOH, KOH, Ca(OH)2, Sr(OH)2; the silicon source is one or more of common silicon sources such as sodium silicate, TEOS, silica sol, fumed silica, macroporous silica gel, etc.; And / or, the salt in step (2) is a soluble sodium salt, preferably one or more of sodium sulfate, sodium nitrate, sodium chloride and sodium fluoride.
7. The method according to claim 1, characterized in that In step (2), the re-crystallization conditions are 20-150° C. for 1-48 hours; preferably, the re-crystallization conditions are 50-120° C. for 5-24 hours; And / or, the mass ratio of the mother liquor to the molecular sieve in step (2) is 1 to 20, preferably 3 to 10; And / or, the recrystallization reaction in step (2) is carried out in a pressurized or non-pressurized closed reaction vessel.
8. A multi-level pore molecular sieve prepared by the method according to any one of claims 1 to 7.
9. The multi-level pore molecular sieve according to claim 8, characterized in that The mesopore volume of the multi-level pore molecular sieve reaches more than 0.20 mL / g, and more than 95% of the micropore volume of the original molecular sieve is retained.
10. The multi-level pore molecular sieve according to claim 8, characterized in that The framework silicon-to-aluminum ratio of the high-silicon mesoporous Y-type molecular sieve is ≥4, more preferably ≥5. Compared with the original molecular sieve, the framework silicon-to-aluminum ratio is increased by more than 20%, more preferably by more than 25%; preferably, the silicon-to-aluminum ratio is increased by less than 80%, more preferably by less than 50%, and most preferably by 30-41%.
Citation Information
Patent Citations
Hierarchical zeolite structure molecular sieve preparation method, prepared molecular sieve and application of molecular sieve
CN109422283A
Hierarchical pore FAU structure molecular sieve and preparation method thereof
CN110937609A
Hierarchical pore HZSM-5 molecular sieve
CN111375441A
Method for preparing hierarchical pore Y-type molecular sieve by modification
CN110950352A
Preparation method of hierarchical porous Y-type molecular sieve
CN118145666A