System and process for producing potassium nitrate and magnesium chloride by double decomposition method

Through multiple purification treatments and electrostatic spraying of anti-corrosion coatings, the problems of by-product purity control and equipment corrosion in potassium nitrate and magnesium chloride processes in metathesis method are solved, and the corrosion resistance of high-purity products and equipment is achieved, and the equipment is extended Service life.

CN119059536APending Publication Date: 2024-12-03SHANDONG HUAYANG DIER CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411431242.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the metathesis method, there are problems in controlling the purity of by-products and high corrosion of equipment in the process of producing potassium nitrate and magnesium chloride, which leads to an increase in maintenance costs.

Method used

Multiple purification treatments are used and anti-corrosion coating is electrostatically sprayed on the inner wall of the synthesis, water washing and resolving kettle. Combined with the nanofiltration membrane to intercept magnesium ions, the superhydrophobic properties of the anti-corrosion coating are used to prevent impurities from adhesion and extend the equipment life.

Benefits of technology

The production of high-purity potassium nitrate and magnesium chloride is achieved, reducing equipment corrosion and extending the equipment service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059536A_ABST
    Figure CN119059536A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of potassium nitrate production, in particular to a system and a process for producing potassium nitrate and magnesium chloride by a double decomposition method, the system comprises a reaction unit, a separation unit and a purification unit, a synthesis kettle of the reaction unit is communicated with filter pressing equipment, and the filter pressing equipment is communicated with a primary crystallization kettle of the separation unit; the primary crystallization kettle is communicated with a first centrifugal machine, the first centrifugal machine is communicated with a second centrifugal machine of the purification unit through a washing kettle, the second centrifugal machine is communicated with a secondary crystallization kettle through a redissolving kettle, and a third centrifugal machine communicated with the secondary crystallization kettle is respectively communicated with the washing kettle and drying equipment. By adopting the structure, potassium nitrate is purified for multiple times, a nanofiltration membrane is arranged in the water washing kettle to intercept magnesium ions, an anti-corrosion coating is electrostatically sprayed on the inner wall of the synthesis kettle to resist nitric acid corrosion, and anti-corrosion coatings are electrostatically sprayed on the inner walls of the synthesis kettle, the water washing kettle and the re-dissolving kettle; impurities are prevented from being attached to the inner wall through the super-hydrophobic performance of the anti-corrosion coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of potassium nitrate production, in particular to a system and process for producing potassium nitrate and magnesium chloride by double decomposition method. Background Art

[0002] The double decomposition method for producing potassium nitrate and magnesium chloride is a chemical process. Its main principle is to react nitric acid with potassium salt (such as potassium chloride) and magnesium chloride with another reagent to exchange ions to obtain the target product. Although this process has its application value, it also has some disadvantages: the process will produce corresponding by-products, and the purity of potassium nitrate needs to be controlled. At the same time, nitric acid in the raw material is a strong acid, which is highly corrosive to production equipment during use, increasing the cost of subsequent maintenance. Summary of the invention

[0003] The object of the present invention is to provide a system and process for producing potassium nitrate and magnesium chloride by double decomposition, wherein potassium nitrate is purified for multiple times, a nanofiltration membrane is arranged in a water washing kettle to intercept magnesium ions, an anti-corrosion coating is electrostatically sprayed on the inner wall of a synthesis kettle to resist nitric acid corrosion, an anti-corrosion coating is electrostatically sprayed on the inner walls of a synthesis kettle, a water washing kettle and a re-dissolution kettle, and the super-hydrophobic property of the anti-corrosion coating is utilized to avoid the attachment of impurities on the inner wall.

[0004] To achieve the above-mentioned purpose, the present invention provides a system for producing potassium nitrate and magnesium chloride by double decomposition method, comprising a reaction unit, a separation unit and a purification unit, wherein the synthesis kettle of the reaction unit is connected with a filter press, the filter press is connected with a primary crystallization kettle of the separation unit, the primary crystallization kettle is connected with a first centrifuge, the first centrifuge is connected with a second centrifuge of the purification unit through a water washing kettle, the second centrifuge is connected with a secondary crystallization kettle through a re-dissolution kettle, and the third centrifuge connected with the secondary crystallization kettle is respectively connected with a water washing kettle and a drying device.

[0005] Preferably, the inner walls of the synthesis kettle, the water washing kettle and the re-dissolving kettle are all electrostatically sprayed with an anti-corrosion coating, and the anti-corrosion coating comprises polydimethylsiloxane, polyvinylidene fluoride, amino-modified multi-walled carbon nanotubes, a silane coupling agent and a solvent.

[0006] Preferably, the solvent includes one or more of N,N-dimethylformamide, tetrahydrofuran and water.

[0007] Preferably, the silane coupling agent includes one or more of silane coupling agent 171, silane coupling agent A172, silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570.

[0008] Preferably, the first centrifuge is communicated with a freezing separation device, and the freezing separation device is respectively communicated with a magnesium chloride storage tank and a primary crystallization kettle.

[0009] The process of the system for producing potassium nitrate and magnesium chloride using the above double decomposition method comprises the following steps: S1. Preparation by double decomposition method: magnesium oxide and nitric acid are put into a synthesis kettle, potassium chloride is slowly added into the synthesis kettle, and the reaction liquid in the synthesis kettle enters a filter press to remove impurities to obtain a de-impurity reaction liquid; S2, separation of potassium nitrate and magnesium chloride: the impurity removal reaction liquid in S1 is subjected to a primary crystallization treatment in a primary crystallization kettle, and after a primary centrifugation in a first centrifuge, the obtained potassium nitrate enters a water washing kettle, the obtained mother liquor enters a freezing separation device for freezing separation, the obtained magnesium chloride solution is canned, and the obtained potassium nitrate is returned to the primary crystallization kettle again, and enters a water washing kettle after passing through the first centrifuge; S3, primary purification of potassium nitrate: the potassium nitrate discharged from the water washing kettle in S2 is centrifuged twice in the second centrifuge, the obtained mother liquor is returned to the reactor, and the obtained potassium nitrate crystals are put into the re-dissolution kettle; S4, secondary purification of potassium nitrate: adding fresh water to the re-dissolution kettle to obtain potassium nitrate solution, which is then crystallized in a secondary crystallization kettle, and the mother liquor obtained by three centrifugations in a third centrifuge is returned to the water washing kettle; S5, drying and packaging: drying and cooling the potassium nitrate crystals obtained by three centrifugations in S4 to obtain a potassium nitrate product, and packaging the finished product; S6, quality inspection and warehousing: The finished products in S5 are quality inspected and put into storage after quality inspection.

[0010] Preferably, in S1, after magnesium oxide and nitric acid are fully reacted, potassium chloride is slowly added to control the pH of the reaction system in the synthesis reactor to be 3-5.

[0011] Preferably, in S1, the molar ratio of nitric acid, magnesium oxide and potassium chloride is 2-3:1-2:2-4.

[0012] Preferably, in S2, the temperature is cooled to 0°C at a rate of 5°C / min in the primary crystallization kettle, and cooled to -20°C to -5°C at a rate of 0.06°C / min in the freezing separation equipment.

[0013] Preferably, in S3, a nanofiltration membrane is provided at the liquid outlet of the washing kettle.

[0014] Preferably, in S4, the temperature in the secondary crystallization kettle is 30-55°C.

[0015] Preferably, the method for preparing the anti-corrosion coating comprises the following steps: T1. Dissolve polydimethylsiloxane (3% by mass) in a solvent mixed with N,N-dimethylformamide and tetrahydrofuran (mass fraction ratio of 1:1), and stir at 80°C for 4 hours; then add polyvinylidene fluoride (2% by mass) to the completely dissolved polydimethylsiloxane solution, and stir magnetically at 70°C for 4 hours to obtain a polyvinylidene fluoride / polydimethylsiloxane solution; T2, adding aminated multi-walled carbon nanotubes to the polyvinylidene fluoride / polydimethylsiloxane solution obtained in T1, and treating with ultrasound at a power of 500 W for 1 hour to obtain a well-dispersed polyvinylidene fluoride / polydimethylsiloxane / aminated multi-walled carbon nanotube mixed solution; T3, hydrolyzing the silane coupling agent to obtain a hydrolyzed silane coupling agent solution for standby use; T4, spray the hydrolyzed silane coupling agent solution in T3 onto the inner wall, and dry it with hot air at 75°C for 0.8h to obtain a semi-cured state; T5. Continue to spray the polyvinylidene fluoride / polydimethylsiloxane / amino-modified multi-walled carbon nanotube mixture in T2 onto the inner wall, set the voltage to 15 kV, and the flow rate to 2.0 mL / h, and obtain an anti-corrosion coating after drying.

[0016] The mechanism of the anti-corrosion coating in the present invention is: The hydrolyzed silane coupling agent is adsorbed on the hydroxyl groups on the inner wall surface, and after hot air drying, it is dehydrated and condensed to form Si-O-Fe bonds, forming a film on the inner wall to facilitate the combination with the amino multi-walled carbon nanotubes in the polyvinylidene fluoride / polydimethylsiloxane / amino multi-walled carbon nanotube mixture, and finally forming an anti-corrosion coating on the inner wall.

[0017] Therefore, the present invention adopts the above-mentioned system and process for producing potassium nitrate and magnesium chloride by double decomposition method, and has the beneficial effects of performing multiple purification treatments on potassium nitrate, and arranging a nanofiltration membrane in the water washing kettle to intercept magnesium ions, so as to obtain high-purity potassium nitrate crystals and a by-product magnesium chloride solution. Meanwhile, the inner walls of the synthesis kettle, the water washing kettle and the re-dissolution kettle are electrostatically sprayed with an anti-corrosion coating to resist nitric acid corrosion, and the super-hydrophobic property prevents impurities from adhering to the inner wall, thereby extending the service life of the synthesis kettle, the water washing kettle and the re-dissolution kettle.

[0018] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic diagram of a system for producing potassium nitrate and magnesium chloride by double decomposition method of the present invention. DETAILED DESCRIPTION

[0020] The present invention is further described below in conjunction with the accompanying drawings and embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0021] Example 1 like Figure 1 As shown, the present invention provides a system for producing potassium nitrate and magnesium chloride by double decomposition method, including a reaction unit, a separation unit and a purification unit. The synthesis kettle of the reaction unit is connected to a filter press, the filter press is connected to a primary crystallization kettle of the separation unit, and the primary crystallization kettle is connected to a first centrifuge. The first centrifuge is connected to the second centrifuge of the purification unit through a water washing kettle, and the second centrifuge is connected to a secondary crystallization kettle through a re-dissolution kettle. The third centrifuge connected to the secondary crystallization kettle is respectively connected to a water washing kettle and a drying device.

[0022] The inner walls of the synthesis kettle, the washing kettle and the re-dissolving kettle are all electrostatically sprayed with an anti-corrosion coating, and the setting of the anti-corrosion coating prevents the corrosion of the inner wall by nitric acid or other substances. At the same time, the super-hydrophobic property of the anti-corrosion coating prevents impurities from adhering to the inner wall. The first centrifuge is connected to the freezing separation equipment, and the freezing separation equipment is respectively connected to the magnesium chloride storage tank and the primary crystallization kettle.

[0023] In the reaction unit, hydrated magnesium nitrate is first obtained, and then potassium nitrate and magnesium chloride are obtained, and a filter press is used to remove impurities in the mother liquor. The mother liquor after impurity removal is separated from potassium nitrate and magnesium chloride in a separation unit, and potassium nitrate is purified in a subsequent purification unit. Potassium nitrate crystals and mother liquor containing potassium nitrate and magnesium chloride are separated in a first centrifuge, and the mother liquor containing potassium nitrate and magnesium chloride enters a freezing separation device, which again separates potassium nitrate crystals and magnesium chloride solution, and the obtained magnesium chloride solution enters a magnesium chloride liquid storage tank, and the obtained potassium nitrate crystals are returned to a primary crystallization kettle again, and enter the first centrifuge for centrifugal operation.

[0024] The potassium nitrate crystals obtained in the first centrifuge enter the water washing kettle, and the potassium nitrate solution obtained is filtered through a nanofiltration membrane after the liquid is discharged, and the divalent magnesium ions are intercepted and returned to the synthesis kettle. The liquid obtained in the second centrifuge returns to the synthesis kettle to participate in the next reaction, and the potassium nitrate crystals obtained enter the re-dissolution kettle, and are heated after adding fresh water. The potassium nitrate solution obtained enters the secondary crystallization kettle, and then potassium nitrate crystals are separated in the third centrifuge, dried in the drying equipment and cooled to obtain the final potassium nitrate crystal finished product packaging, and the obtained secondary mother liquor returns to the water washing kettle.

[0025] Example 2 The process of a system for producing potassium nitrate and magnesium chloride using the above-mentioned double decomposition method includes the following steps: S1, double decomposition method preparation: magnesium oxide and nitric acid are put into a synthesis kettle, potassium chloride is slowly added to the synthesis kettle, and the reaction liquid in the synthesis kettle enters a filter press to remove impurities to obtain a de-impurity reaction liquid.

[0026] In S1, the molar ratio of nitric acid, magnesium oxide and potassium chloride is 2-3:1-2:2-4.

[0027] In S1, after magnesium oxide and nitric acid are fully reacted, potassium chloride is added to control the pH of the reaction system in the synthesis reactor to be 3-5.

[0028] S2, separation of potassium nitrate and magnesium chloride: the impurity removal reaction liquid in S1 is subjected to a crystallization treatment in a primary crystallization kettle, and after a centrifugation in a first centrifuge, the obtained potassium nitrate enters a water washing kettle, the obtained mother liquor enters a freezing separation device for freezing separation, the obtained magnesium chloride solution is canned, and the obtained potassium nitrate is returned to the primary crystallization kettle again, and enters a water washing kettle after passing through the first centrifuge.

[0029] In S2, the temperature is lowered to 0°C at a rate of 5°C / min in the primary crystallization kettle, and to -20°C to -5°C at a rate of 0.06°C / min in the freezing separation equipment. Potassium nitrate crystals with a moderate particle size are obtained in the freezing separation equipment to avoid the potassium nitrate crystals being too large to form agglomerates or too small to be easily separated from the magnesium chloride solution.

[0030] S3, primary purification of potassium nitrate: The potassium nitrate discharged from the water washing kettle in S2 is centrifuged twice in the second centrifuge, the obtained mother liquor is returned to the reactor, and the obtained potassium nitrate crystals are put into the re-dissolution kettle.

[0031] In S3, a nanofiltration membrane is provided at the liquid outlet of the water washing kettle to intercept and separate the magnesium ions in the potassium nitrate solution, and potassium nitrate and potassium chloride are separated again in the subsequent reaction.

[0032] S4. Secondary purification of potassium nitrate: fresh water is added to the re-dissolution kettle to obtain potassium nitrate solution, which is then crystallized in a secondary crystallization kettle. The mother liquor obtained by three centrifugations in a third centrifuge is returned to the water washing kettle.

[0033] In S4, the temperature in the secondary crystallization kettle is 30-55°C.

[0034] S5, drying and packaging: drying and cooling the potassium nitrate crystals obtained by three centrifugations in S4 to obtain a potassium nitrate product, and packaging the finished product.

[0035] S6, quality inspection and warehousing: The finished products in S5 are quality inspected and put into storage after quality inspection.

[0036] Example 3 The inner walls of the synthesis kettle, the water washing kettle and the re-dissolving kettle are all electrostatically sprayed with an anti-corrosion coating, and the anti-corrosion coating comprises polydimethylsiloxane, polyvinylidene fluoride, amino multi-walled carbon nanotubes, a silane coupling agent and a solvent.

[0037] The solvent includes one or more of N,N-dimethylformamide, tetrahydrofuran and water.

[0038] The method for preparing the anti-corrosion coating in Example 1 comprises the following steps: T1. Dissolve polydimethylsiloxane (3% by mass) in a mixed solvent of N,N-dimethylformamide and tetrahydrofuran (mass fraction ratio of 1:1) and stir at 80°C for 4 hours. Then, add polyvinylidene fluoride (2% by mass) to the completely dissolved polydimethylsiloxane solution and stir magnetically at 70°C for 4 hours to obtain a polyvinylidene fluoride / polydimethylsiloxane solution.

[0039] T2. Adding aminated multi-walled carbon nanotubes to the polyvinylidene fluoride / polydimethylsiloxane solution obtained in T1, and continuously treating with ultrasound at a power of 500 W for 1 hour to obtain a well-dispersed polyvinylidene fluoride / polydimethylsiloxane / aminated multi-walled carbon nanotube mixed solution.

[0040] T3, hydrolyzing the silane coupling agent to obtain a hydrolyzed silane coupling agent solution for standby use.

[0041] T4. Spray the hydrolyzed silane coupling agent solution in T3 onto the inner wall and dry it with hot air at 75°C for 0.8h to obtain a semi-cured state.

[0042] T5. Continue to spray the polyvinylidene fluoride / polydimethylsiloxane / amino-modified multi-walled carbon nanotube mixture in T2 onto the inner wall, set the voltage to 15 kV, and the flow rate to 2.0 mL / h, and obtain an anti-corrosion coating after drying.

[0043] Therefore, the present invention adopts the above-mentioned system and process for producing potassium nitrate and magnesium chloride by double decomposition, performs multiple purification treatments on potassium nitrate, and arranges a nanofiltration membrane in a water washing kettle to intercept magnesium ions, so as to obtain high-purity potassium nitrate crystals and a by-product magnesium chloride solution. Meanwhile, the inner walls of the synthesis kettle, the water washing kettle and the re-dissolution kettle are electrostatically sprayed with an anti-corrosion coating to resist nitric acid corrosion, and the super-hydrophobic property prevents impurities from adhering to the inner wall, thereby extending the service life of the synthesis kettle, the water washing kettle and the re-dissolution kettle.

[0044] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A system for producing potassium nitrate and magnesium chloride by double decomposition, characterized in that: The invention comprises a reaction unit, a separation unit and a purification unit, wherein the synthesis kettle of the reaction unit is connected with a filter press, the filter press is connected with a primary crystallization kettle of the separation unit, the primary crystallization kettle is connected with a first centrifuge, the first centrifuge is connected with a second centrifuge of the purification unit through a water washing kettle, the second centrifuge is connected with a secondary crystallization kettle through a re-dissolution kettle, and the third centrifuge connected with the secondary crystallization kettle is respectively connected with a water washing kettle and a drying device.

2. A system for producing potassium nitrate and magnesium chloride by double decomposition according to claim 1, characterized in that: The inner walls of the synthesis kettle, the water washing kettle and the re-dissolving kettle are all electrostatically sprayed with an anti-corrosion coating, and the anti-corrosion coating comprises polydimethylsiloxane, polyvinylidene fluoride, amino multi-walled carbon nanotubes, a silane coupling agent and a solvent.

3. A system for producing potassium nitrate and magnesium chloride by double decomposition according to claim 2, characterized in that: The solvent includes one or more of N,N-dimethylformamide, tetrahydrofuran and water.

4. A system for producing potassium nitrate and magnesium chloride by double decomposition according to claim 1, characterized in that: The first centrifuge is communicated with the freezing separation equipment, and the freezing separation equipment is respectively communicated with the magnesium chloride storage tank and the primary crystallization kettle.

5. A process for producing potassium nitrate and magnesium chloride using a system for producing potassium nitrate and magnesium chloride using a double decomposition method according to any one of claims 1 to 4, characterized in that: The following steps are included: S1. Preparation by double decomposition method: magnesium oxide and nitric acid are put into a synthesis kettle, potassium chloride is slowly added into the synthesis kettle, and the reaction liquid in the synthesis kettle enters a filter press to remove impurities to obtain a de-impurity reaction liquid; S2, separation of potassium nitrate and magnesium chloride: the impurity removal reaction liquid in S1 is subjected to a primary crystallization treatment in a primary crystallization kettle, and after a primary centrifugation in a first centrifuge, the obtained potassium nitrate enters a water washing kettle, the obtained mother liquor enters a freezing separation device for freezing separation, the obtained magnesium chloride solution is canned, and the obtained potassium nitrate is returned to the primary crystallization kettle again, and enters a water washing kettle after passing through the first centrifuge; S3, primary purification of potassium nitrate: the potassium nitrate discharged from the water washing kettle in S2 is centrifuged twice in the second centrifuge, the obtained mother liquor is returned to the reactor, and the obtained potassium nitrate crystals are put into the re-dissolution kettle; S4, secondary purification of potassium nitrate: adding fresh water to the re-dissolution kettle to obtain potassium nitrate solution, which is then crystallized in a secondary crystallization kettle, and the mother liquor obtained by three centrifugations in a third centrifuge is returned to the water washing kettle; S5, drying and packaging: drying and cooling the potassium nitrate crystals obtained by three centrifugations in S4 to obtain a potassium nitrate product, and packaging the finished product; S6, quality inspection and warehousing: The finished products in S5 are quality inspected and put into storage after quality inspection.

6. A process for producing potassium nitrate and magnesium chloride using a double decomposition process according to claim 5, characterized in that: In S1, after magnesium oxide and nitric acid are fully reacted, potassium chloride is slowly added to control the pH of the reaction system in the synthesis reactor to 3-5.

7. The process of a system for producing potassium nitrate and magnesium chloride using a double decomposition process according to claim 5, characterized in that: In S1, the molar ratio of nitric acid, magnesium oxide and potassium chloride is 2-3:1-2:2-4.

8. The process of a system for producing potassium nitrate and magnesium chloride using double decomposition according to claim 5, characterized in that: In S2, the temperature is lowered to 0°C at a rate of 5°C / min in the primary crystallization kettle, and to -20°C to -5°C at a rate of 0.06°C / min in the freezing separation equipment.

9. The process of a system for producing potassium nitrate and magnesium chloride using double decomposition according to claim 5, characterized in that: In S3, a nanofiltration membrane is provided at the liquid outlet of the washing kettle.

10. The process of a system for producing potassium nitrate and magnesium chloride using double decomposition according to claim 5, characterized in that: In S4, the temperature in the secondary crystallization kettle is 30-55°C.