Preparation method and application of perovskite type ceramic material with high infrared emissivity

Through sol-gel method and discharge plasma sintering technology, high-density perovskite ceramic materials were prepared, solving the problem of insufficient infrared emission performance of traditional ceramic materials, and achieving high purity and high-efficiency infrared emission performance ceramic materials.

CN119059805AActive Publication Date: 2024-12-03INNER MONGOLIA UNIV OF TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411193152.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

Traditional ceramic materials have limitations in infrared emission performance and are difficult to meet the growing application needs.

Method used

Perovskite-type ceramic materials were prepared by sol-gel method. The combination of rare earth elements, alkaline earth metal elements and transition metal elements was used to prepare an aqueous solution using nitrate as raw material, and the dry gel was formed through a water bath. Then, the horse was used to make a Fur furnace and discharge plasma sintering technology to prepare high-density ceramic blocks.

Benefits of technology

It realizes high purity, high density and excellent infrared emission performance of ceramic materials, improves the infrared emissivity and fracture toughness of the materials, and is suitable for infrared radiation and detection fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059805A_ABST
    Figure CN119059805A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a perovskite type ceramic material with high infrared emissivity, and the preparation method comprises the following steps: weighing each solid nitrate according to the molar ratio of the chemical formula (La0. 2Y0. 2Sm0. 2M10. 2M0. 2) (Cr1-xAex) O3 (x = 0-0.5), adding deionized water to prepare a solution A, adding a chelating agent into the solution A, stirring to obtain a solution A1, adding a dispersing agent into the solution B, stirring to obtain a solution A2, filtering, washing, and drying to obtain the perovskite type ceramic material with high infrared emissivity. Adjusting the pH value of the solution A2 to 7-9 to obtain a solution A3, heating the solution A3 in a water bath for 1-2 hours to obtain a solution A4, drying the solution A4 at 90-120 DEG C to obtain xerogel, grinding the xerogel to obtain powder B, calcining the ground powder B by using a muffle furnace to obtain precursor powder C, and calcining the precursor powder C by using a muffle furnace to obtain precursor powder B; and placing the graphite mold filled with the precursor powder C in a discharge plasma sintering furnace cavity for sintering to obtain the LaCrO3-based ceramic block material with high infrared emissivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic materials, in particular to a preparation method and application of a perovskite-type ceramic material with high infrared emissivity. Background Art

[0002] In the rapid development of modern science and technology, the importance of materials science as the cornerstone of many high-tech fields is self-evident. Especially under extreme working conditions such as high temperature, high radiation, and high energy efficiency, the performance requirements of materials are becoming more and more stringent. As one of the key indicators of the thermal radiation characteristics of materials, infrared emission performance is of great significance for improving energy utilization efficiency, enhancing the performance of thermal management systems, and developing new infrared stealth technologies.

[0003] Although traditional ceramic materials have excellent properties such as high temperature resistance and corrosion resistance, they often have limitations in infrared emission performance and cannot meet the growing application needs. Therefore, the development of new ceramic materials with high infrared emissivity has become an important direction of materials science research. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a preparation method and application of a perovskite ceramic material with high infrared emissivity.

[0005] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing a perovskite ceramic material with high infrared emissivity, comprising:

[0006] (1) According to the chemical formula (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )O3 (x = 0 to 0.5), weigh La(NO3)3·6H2O, Y(NO3)3·6H2O, Sm(NO3)3·6H2O, M(NO3)3·6H2O or M(NO3)3·4H2O, Cr(NO3)3·9H2O, and Ae(NO3)2·3H2O, and add them into deionized water in sequence to prepare nitric acid aqueous solution A, stirring the whole process and heating in a water bath, wherein M is a rare earth element or an alkaline earth metal element, and Ae is a transition metal element;

[0007] (2) adding a chelating agent to the nitric acid aqueous solution A and stirring thoroughly to obtain a solution A1;

[0008] (3) adding a dispersant to solution B and stirring thoroughly to obtain solution A2;

[0009] (4) After stirring for 0.5 h to 1.0 h, add aqueous ammonia to solution A2 to adjust the pH value to 7 to 9 to obtain solution A3;

[0010] (5) Solution A3 is further heated in a water bath for 1 h to 2 h to obtain solution A4;

[0011] (6) continuously drying the solution A4 at 90° C. to 120° C. until a dry gel is obtained, and grinding the dry gel to obtain powder B;

[0012] (7) calcining the ground powder B using a muffle furnace to obtain a precursor powder C;

[0013] (8) Placing the graphite mold filled with the precursor powder C in a spark plasma sintering furnace chamber for sintering, and obtaining a ceramic block after sintering.

[0014] As a further improvement of the present invention: M1 and M2 in the chemical formula of step (1) are any one of Ce, Pr, Nd, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Mg, Ca, Sr, and Ba.

[0015] As a further improvement of the present invention: Ae in the chemical formula of step (1) is any one of Ti, Mn, Fe, Co, Ni, Cu, and Zn.

[0016] As a further improvement of the present invention: in steps (1) to (5), the stirring speed is 500 r / min to 1000 r / min, and the water bath heating temperature is 80° C. to 90° C.

[0017] As a further improvement of the present invention: in step (2), the chelating agent is any one of citric acid, ethylenediaminetetraacetic acid, glycine, and acrylic acid, and the amount of the chelating agent is (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )The molar ratio of all metal ions in O3 is 1.2 to 1.5:1.

[0018] As a further improvement of the present invention: in step (3), the dispersant is ethylene glycol or polyvinyl alcohol, and the amount of the dispersant is (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )The molar ratio of all metal ions in O3 is 3 to 4:1.

[0019] As a further improvement of the present invention: in step (7), the sintering temperature of the muffle furnace is 450° C. to 550° C., the holding time is 5 h to 10 h, the heating rate is 2° C. / min, and the precursor powder C is obtained after natural cooling.

[0020] As a further improvement of the present invention: in step (8), the heating rate of the spark plasma sintering furnace chamber is 50°C / min to 100°C / min, the insulation temperature is 1300°C to 1500°C, and the insulation time is 5min to 10min.

[0021] The present invention also applies the ceramic block material prepared by the above preparation method to the preparation of infrared radiation materials.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention combines rare earth elements, alkaline earth metal elements and transition metal elements, uses various metal nitrates as raw materials to prepare aqueous solution A, uses a sol-gel method to prepare dry gel B, sinters to obtain precursor powder C, and uses spark plasma sintering technology to sinter the precursor powder C to prepare high-density ceramic block D, thereby achieving high purity, high density and excellent infrared emission performance of the material.

[0024] The present invention adopts a sol-gel method as a preparation method of a precursor, which can ensure that the raw materials are uniformly mixed at the molecular or atomic level, thereby preparing a dry gel B with uniform composition and fine particle size. The method has the advantages of simple operation, mild conditions, high product purity, etc., and is conducive to the formation of high-quality ceramic blocks in the subsequent sintering process. After sintering, impurities and organic residues in the dry gel can be effectively discharged to obtain a pure precursor powder C, thereby improving the purity and performance of the ceramic material. The precursor powder C is quickly sintered by using a spark plasma sintering technology, and a high temperature can be reached in a short time to densify the ceramic material, thereby preparing a highly dense ceramic block D, which is conducive to maintaining the microstructure and stable performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is (La prepared in Example 1 of the present invention 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )Microscopic morphology of CrO3 ceramic block.

[0026] Figure 2 is the (La prepared in Example 2 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )(Cr 0.8 Cu0.2 )Microscopic morphology of O3 material.

[0027] Figure 3 is the (La prepared in Example 3 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )(Cr 0.7 Cu 0.3 )Microscopic morphology of O3 ceramic block.

[0028] Figure 4 is (La prepared in Examples 1 to 3 of the present invention 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x ) Vickers hardness diagram of O3 (x=0~0.5) material.

[0029] Figure 5 is (La prepared in Examples 1 to 3 of the present invention 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )Fracture toughness diagram of O3 (x=0~0.5) material.

[0030] Figure 6 is (La prepared in Examples 1 to 3 of the present invention 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )Room temperature infrared emissivity diagram of O3 (x=0~0.5) ceramic material in 3-5μm and 8-14μm bands. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0032] In order to solve the technical problems in the prior art, the present invention is further described in conjunction with the accompanying drawings and embodiments:

[0033] like Figures 1 to 6 As shown, the present invention discloses a method for preparing a perovskite ceramic material with high infrared emissivity, comprising:

[0034] Step (1), according to the chemical formula (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )O3 (x = 0 to 0.5), namely, La(NO3)3·6H2O, Y(NO3)3·6H2O, Sm(NO3)3·6H2O, M(NO3)3·6H2O or M(NO3)3·4H2O, Cr(NO3)3·9H2O, Ae(NO3)2·3H2O are weighed, and added into deionized water in sequence to prepare nitric acid aqueous solution A, with stirring and water bath heating throughout the process, wherein M is a rare earth element or an alkaline earth metal element, and Ae is a transition metal element;

[0035] Specifically, in step (1), the molar ratio of La(NO3)3·6H2O, Y(NO3)3·6H2O, Sm(NO3)3·6H2O, M(NO3)3·6H2O or M(NO3)2·4H2O, Cr(NO3)3·9H2O, and Ae(NO3)2·3H2O is 0.2:0.2:0.2:0.2:1-x:x. Weigh two portions of M(NO3)3·6H2O or M(NO3)2·4H2O.

[0036] The purity of La(NO3)3·6H2O, Y(NO3)3·6H2O, Sm(NO3)3·6H2O, M(NO3)3·6H2O or M(NO3)2·4H2O, Cr(NO3)3·9H2O, and Ae(NO3)2·3H2O is 99%.

[0037] Step (2), adding a chelating agent to the nitric acid aqueous solution A and stirring thoroughly to obtain a solution A1;

[0038] Step (3), adding a dispersant to solution B and stirring thoroughly to obtain solution A2;

[0039] Step (4), after stirring for 0.5 h to 1.0 h, add aqueous ammonia to solution A2 to adjust the pH value to 7 to 9 to obtain solution A3;

[0040] Step (5), heating solution A3 in a water bath for 1 h to 2 h to obtain solution A4;

[0041] Step (6), drying the solution E at 90° C. to 120° C. until a dry gel is obtained, and grinding the dry gel to obtain powder B;

[0042] Step (7), calcining the ground powder B using a muffle furnace, and obtaining a precursor powder C after sintering;

[0043] Step (8), placing the graphite mold filled with the precursor powder C in a spark plasma sintering furnace chamber for sintering, and obtaining a ceramic block after the sintering is completed.

[0044] Further, step (1) chemical formula (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )O3 (x = 0 ~ 0.5) where M1 and M2 are any one of Ce, Pr, Nd, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Mg, Ca, Sr, and Ba respectively.

[0045] In other words, the chemical formula (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )O3 (x = 0 ~ 0.5), the solid nitrate containing M1 and M2 can be M(NO3)3·6H2O or M(NO3)3·4H2O. Specifically, M in M(NO3)3·6H2O or M(NO3)3·4H2O is a rare earth element or an alkaline earth metal element, and M is specifically any one of Ce, Pr, Nd, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Mg, Ca, Sr, and Ba.

[0046] Further, step (1) chemical formula (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )Ae in O3 (x=0~0.5) is any one of Ti, Mn, Fe, Co, Ni, Cu, and Zn.

[0047] Furthermore, in steps (1) to (5), the stirring speed is 500 r / min to 1000 r / min, and the water bath heating temperature is 80° C. to 90° C.

[0048] Furthermore, in step (5), the water bath is heated for 1 h to 2 h.

[0049] Wherein, the chelating agent in step (2) is any one of citric acid, ethylenediaminetetraacetic acid, glycine, and acrylic acid, and the ratio of the amount of the chelating agent to the amount of all metal ions is 1.2 to 1.5:1, that is, the amount of the chelating agent is 1.2 to 1.5:1. 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )The molar ratio of all metal ions in O3 is 1.2 to 1.5:1 to form a stable complex and ensure the uniformity and stability of sol formation.

[0050] In step (3), the dispersant is ethylene glycol or polyvinyl alcohol, and the amount of the dispersant is (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )The molar ratio of all metal ions in O3 is 3.6-4.5:1, which makes the sol evenly dispersed and prevents agglomeration.

[0051] In addition, ammonia water is used as a catalyst and pH regulator to adjust the pH value of the solution to 7-9, accelerating the hydrolysis and polycondensation reactions in the sol-gel method.

[0052] In step (6), the dry gel is ground into powder or fine particles using an agate mortar to reduce the particle size, increase the specific surface area, and improve the uniformity and consistency of the material.

[0053] In step (7), the gel powder B in step (6) is placed to one third to one half of the crucible to prevent the gel from expanding and escaping due to heat. The sintering temperature of the muffle furnace is 500°C, the holding time is 5h to 10h, the heating rate is 2°C / min, and the precursor powder C is obtained after natural cooling. The purpose of pre-sintering is to form a precursor powder accompanied by the release of decomposition gas, and to remove incompletely reacted nitrates, organic residues, etc., to improve the purity of the product.

[0054] In step (8), the heating rate of the spark plasma sintering furnace chamber is 50°C / min to 100°C / min, the holding temperature is 1300°C to 1500°C, and the holding time is 5min to 10min. After sintering, a ceramic block (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er0.2 )CrO3.

[0055] The present invention adopts a high entropy design concept, and increases the configuration entropy of the material by introducing a variety of elements (rare earth elements such as La, Y, Sm, as well as alkaline earth metal elements M and transition metal elements Ae) to form a complex solid solution. Specifically, aqueous solution A is prepared using various metal nitrates as raw materials, and dry gel B is prepared using a sol-gel method. The precursor powder C is obtained by sintering at 500°C to remove impurities, and then the precursor powder C is sintered using a spark plasma sintering technique to prepare a highly dense ceramic block D. Combining multiple rare earth, alkaline earth metal and transition metal elements, the material has high purity, high density and excellent infrared emission performance, and has broad application prospects in the fields of infrared radiation heating, infrared detection and the like.

[0056] At the same time, the combination of multiple elements makes the material more adjustable and has greater room for optimization in terms of performance. The perovskite structure (ABO3) has good stability and thermal performance. By adjusting the types and proportions of the A- and B-site elements, the infrared emissivity and other properties of the material can be further adjusted.

[0057] The present invention adopts the sol-gel method as the preparation method of the precursor, which can ensure that the raw materials are uniformly mixed at the molecular or atomic level, so as to prepare a dry gel B with uniform composition and fine particle size. The method has the advantages of simple operation, mild conditions, and high product purity, which is helpful to form high-quality ceramic blocks in the subsequent sintering process. After low-temperature sintering at 500°C, impurities and organic residues in the dry gel can be effectively discharged to obtain a pure precursor powder C. This step is very important for improving the purity and performance of ceramic materials. The precursor powder C is quickly sintered using spark plasma sintering technology, which can reach a high temperature and densify the ceramic material in a short time, thereby preparing a highly dense ceramic block D, which helps to maintain the microstructure and stable performance of the material.

[0058] The infrared emissivity of LaCrO3-based ceramic block D between room temperature and 600°C is 0.783-0.955 in the 3-5μm range and 0.924-0.979 in the 8-14μm band, which is more than 30% higher than the infrared emissivity of pure LaCrO3. Its fracture toughness is 0.87MPa·m1 / 2-1.55MPa·m1 / 2, and its microhardness is 9.14GPa-15.23GPa, which is 1.91GPa-8.00GPa higher than the microhardness of pure LaCrO3.

[0059] Embodiment 1

[0060] This embodiment provides a method for preparing a perovskite ceramic material with high infrared emissivity, comprising:

[0061] Step (1), according to the ceramic chemical formula (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )CrO3 in a molar ratio of 0.2:0.2:0.2:0.2:0.2:1, and various solid nitrates were weighed, namely, La(NO3)3·6H2O, Y(NO3)3·6H2O, Sm(NO3)3·6H2O, Eu(NO3)3·6H2O, Er(NO3)3·6H2O, and Cr(NO3)3·9H2O. The molar ratio of the solid nitrates was 0.2:0.2:0.2:0.2:0.2:1, and the solid nitrates were added into deionized water in turn to prepare nitric acid aqueous solution A, with stirring and heating in a water bath throughout the process;

[0062] Step (2), adding 0.24 mol of citric acid to the nitric acid aqueous solution A and stirring thoroughly to obtain solution A1;

[0063] Step (3), adding 0.72 mol of ethylene glycol to solution B and stirring thoroughly to obtain solution A2;

[0064] Step (4), after stirring for 0.5 h, NH3·H2O was added to solution A2 to adjust the pH value to 7-9 to obtain solution A3.

[0065] Step (5), heating solution A3 in a water bath for 1.5 h to obtain solution A4;

[0066] Step (6), drying the solution A4 at 100° C. until a dry gel is obtained, and grinding the dry gel to obtain powder B;

[0067] Step (7), calcining the ground powder B in a muffle furnace, and obtaining a precursor powder C after sintering; wherein the sintering rate is 2°C / min, the sintering temperature is 500°C, and the holding time is 5h;

[0068] Step (8), placing the graphite mold containing the precursor powder C in a spark plasma sintering furnace chamber for sintering, the heating rate is 100 ° C / min, the holding temperature is 1300 ° C, the holding time is 5 min, and the sintering is completed to obtain a ceramic block (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )CrO3.

[0069] Figure 1 The high entropy (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2) Microscopic morphology of CrO3 infrared radiation ceramic block. It can be seen from the figure that it is uniform short rod-shaped particles. The preparation method of this embodiment can refine the grains and inhibit grain growth, so that the product has a high density.

[0070] like Figure 4 As shown in Sample 1, its microhardness is 9.14 GPa. Figure 5 As shown in Sample 1, its fracture toughness is 0.87MPa·m1 / 2; Figure 6 As shown in Sample 1, in this embodiment, the infrared emissivity of the ceramic block in the 3-5 μm band at room temperature is 0.783, and the infrared emissivity of the 8-14 μm band is 0.969.

[0071] Example 2

[0072] This embodiment provides a method for preparing a perovskite ceramic material with high infrared emissivity, comprising:

[0073] Step (1), according to the ceramic chemical formula (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )(Cr 0.8 Cu 0.2 )O3, namely, La(NO3)3·6H2O, Y(NO3)3·6H2O, Sm(NO3)3·6H2O, Eu(NO3)3·6H2O, Er(NO3)3·6H2O, Cr(NO3)3·9H2O, and Cu(NO3)2·3H2O with a molar ratio of 0.2:0.2:0.2:0.2:0.2:0.8:0.2, and add them into deionized water in turn to prepare nitric acid aqueous solution A, stirring the whole process and heating in a water bath.

[0074] Step (2), add 0.25 mol of citric acid to solution A and stir thoroughly to obtain solution A1.

[0075] Step (3), add 0.75 mol of ethylene glycol to solution A1 and stir thoroughly to obtain solution A2.

[0076] Step (4), after stirring for 0.5 h, NH3·H2O was added to solution A2 to adjust the pH to 7 to obtain solution A3.

[0077] Step (5), heating solution A3 in a water bath for 1.5 h to obtain solution A4.

[0078] Step (6), drying the solution A4 at 100° C. until a dry gel is obtained, and grinding the dry gel to obtain powder B.

[0079] Step (7), calcining the ground powder B using a muffle furnace, and obtaining a precursor powder C after sintering, wherein the sintering rate is 2°C / min, the sintering temperature is 500°C, and the holding time is 5h.

[0080] Step (8), placing the graphite mold containing the precursor powder C in a spark plasma sintering furnace chamber for sintering, the heating rate is 100 ° C / min, the holding temperature is 1300 ° C, the holding time is 5 min, and the sintering is completed to obtain a ceramic block (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )(Cr 0.8 Cu 0.2 )O3.

[0081] from Figure 2 It can be seen that (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )(Cr 0.8 Cu 0.2 )O3 ceramics are uniform short rod-shaped particles. Figure 4 As shown in Sample 2, its microhardness is 13.97 GPa. Figure 5 Sample 2 shows that its fracture toughness is 1.45 MPa·m 1 / 2 ;like Figure 6 As shown in Sample 2 of this embodiment, the infrared emissivity of the ceramic block in the 3-5 μm band at room temperature is 0.813, and the infrared emissivity of the 8-14 μm band is 0.962.

[0082] Embodiment 3

[0083] This embodiment provides a method for preparing a perovskite ceramic material with high infrared emissivity, comprising:

[0084] Step (1), according to the ceramic chemical formula (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )(Cr 0.7 Cu 0.3)O3, namely, La(NO3)3·6H2O, Y(NO3)3·6H2O, Sm(NO3)3·6H2O, Eu(NO3)3·6H2O, Er(NO3)3·6H2O, Cr(NO3)3·9H2O, and Cu(NO3)2·3H2O with a molar ratio of 0.2:0.2:0.2:0.2:0.2:0.7:0.3, and added them into deionized water in turn to prepare nitric acid aqueous solution A, stirring the whole process and heating in a water bath.

[0085] Step (2), adding 0.24 mol of citric acid to solution A and stirring thoroughly to obtain solution A1;

[0086] Step (3), adding 0.72 mol of ethylene glycol to solution A1 and stirring thoroughly to obtain solution A2;

[0087] Step (4), after stirring for 0.5 h, adding aqueous ammonia to solution A2 to adjust the pH to 7 to obtain solution A3;

[0088] Step (5), heating solution A3 in a water bath for 1.5 h to obtain solution A4;

[0089] Step (6), heating the solution A4 in a drying oven at 90° C. for 12 h, and then drying at 120° C. until a dry gel is obtained, and grinding the dry gel to obtain powder B;

[0090] Step (7), calcining the ground powder B in a muffle furnace, and obtaining the precursor powder C after sintering. The sintering rate is 2°C / min, the sintering temperature is 500°C, and the holding time is 5h.

[0091] Step (8), placing the graphite mold containing the precursor powder C in a spark plasma sintering furnace chamber for sintering, the heating rate is 100°C / min, the holding temperature is 1400°C, the holding time is 5min, and the sintering is completed to obtain a ceramic block (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )(Cr 0.7 Cu 0.3 )O3.

[0092] from Figure 3 It can be seen that (La 0.2 Y 0.2 Sm 0.2 Eu 0.2 Er 0.2 )(Cr 0.7 Cu 0.3 )O3 ceramics are uniform short rod-shaped particles. Figure 4 As shown in Sample 3, its microhardness is 15.23 GPa. Figure 5 Sample 3 shows that its fracture toughness is 1.55 MPa·m 1 / 2 ;like Figure 4 As shown in Sample 3 of this embodiment, the infrared emissivity of the ceramic block in the 3-5 μm band at room temperature is 0.832, and the infrared emissivity of the 8-14 μm band is 0.959.

[0093] In summary, after reading the present invention document, ordinary technicians in this field can make other various corresponding transformation schemes based on the technical scheme and technical concept of the present invention without creative mental work, which all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a perovskite ceramic material with high infrared emissivity, characterized in that: The following steps are involved: (1) According to the chemical formula (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )O3 (x = 0 to 0.5), weigh La(NO3)3·6H2O, Y(NO3)3·6H2O, Sm(NO3)3·6H2O, M(NO3)3·6H2O or M(NO3)3·4H2O, Cr(NO3)3·9H2O, and Ae(NO3)2·3H2O, and add them into deionized water in sequence to prepare nitric acid aqueous solution A, stirring the whole process and heating in a water bath, wherein M is a rare earth element or an alkaline earth metal element, and Ae is a transition metal element; (2) adding a chelating agent to the nitric acid aqueous solution A and stirring thoroughly to obtain a solution A1; (3) adding a dispersant to solution B and stirring thoroughly to obtain solution A2; (4) After stirring for 0.5 h to 1.0 h, add aqueous ammonia to solution A2 to adjust the pH value to 7 to 9 to obtain solution A3; (5) Solution A3 is further heated in a water bath for 1 h to 2 h to obtain solution A4; (6) continuously drying the solution A4 at 90° C. to 120° C. until a dry gel is obtained, and grinding the dry gel to obtain powder B; (7) calcining the ground powder B using a muffle furnace to obtain a precursor powder C; (8) Placing the graphite mold filled with the precursor powder C in a spark plasma sintering furnace chamber for sintering, and obtaining a ceramic block after sintering.

2. The method for preparing a perovskite ceramic material with high infrared emissivity according to claim 1, characterized in that: In step (1), M1 and M2 in the chemical formula are any one of Ce, Pr, Nd, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Mg, Ca, Sr, and Ba.

3. The method for preparing a perovskite ceramic material with high infrared emissivity according to claim 1, characterized in that: Ae in the chemical formula of step (1) is any one of Ti, Mn, Fe, Co, Ni, Cu and Zn.

4. The method for preparing a perovskite ceramic material with high infrared emissivity according to claim 1, characterized in that: In steps (1) to (5), the stirring speed is 500 r / min to 1000 r / min, and the water bath heating temperature is 80° C. to 90° C.

5. The method for preparing a perovskite ceramic material with high infrared emissivity according to claim 1, characterized in that: In step (2), the chelating agent is any one of citric acid, ethylenediaminetetraacetic acid, glycine, and acrylic acid, and the amount of the chelating agent is (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1-x Ae x )The molar ratio of all metal ions in O3 is 1.2 to 1.5:

1.

6. The method for preparing a perovskite ceramic material with high infrared emissivity according to claim 1, characterized in that: In step (3), the dispersant is ethylene glycol or polyvinyl alcohol, and the amount of the dispersant is (La 0.2 Y 0.2 Sm 0.2 M1 0.2 M2 0.2 )(Cr 1- x Ae x )The molar ratio of all metal ions in O3 is 3 to 4:

1.

7. The method for preparing a perovskite ceramic material with high infrared emissivity according to claim 1, characterized in that: In step (7), the sintering temperature of the muffle furnace is 450° C. to 550° C., the holding time is 5 h to 10 h, the heating rate is 2° C. / min, and the precursor powder C is obtained after natural cooling.

8. The method for preparing a perovskite ceramic material with high infrared emissivity according to claim 1, characterized in that: In step (8), the heating rate of the spark plasma sintering furnace chamber is 50°C / min to 100°C / min, the insulation temperature is 1300°C to 1500°C, and the insulation time is 5min to 10min.

9. Use of the ceramic block according to any one of claims 1 to 8 in the preparation of infrared radiation materials.

Citation Information

Patent Citations

  • High-emissivity infrared energy-saving high-entropy material with perovskite structure and preparation method thereof

    CN113149088A

  • Preparation method and application of B-site pentabasic high-entropy perovskite catalyst

    CN113171779A

  • High-infrared-emissivity perovskite type ceramic material and preparation method and application thereof

    CN117534460A

  • High-entropy perovskite type thermal sensitive ceramic with high temperature and negative temperature coefficient as well as preparation method and application of thermal sensitive ceramic

    CN117776692A