Method for preparing unsaturated nitrile

By reacting carbon-carbon double bond aldehyde with ammonia and nitrogen under oxygen-free conditions, a simple catalyst design is used to solve the problems of hydrocyanic acid generation, temperature control and catalyst complexity in unsaturated nitrile synthesis, achieving high efficiency, Environmentally friendly production of unsaturated nitrile.

CN119059932APending Publication Date: 2024-12-03SHANGHAI HUAYI NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411158902.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing unsaturated nitrile synthesis process has problems such as the formation of highly toxic byproducts, the strong exothermic process, the difficulty in temperature control, the complex catalyst design and high cost, and the byproducts have no commercial value.

Method used

Under oxygen-free conditions, the reactor containing a catalyst reacts the aldehyde of the carbon-carbon double bond with a mixed gas of ammonia and nitrogen to form unsaturated nitrile. The catalyst consists of supported metal elements and supports, and the reaction temperature is between 250-450°C , the pressure is between 1-5 atmospheres, avoiding the participation of oxidants, and use water vapor and ammonia for continuous reaction.

Benefits of technology

The formation of hydrogen cyanide is avoided, the selectivity and conversion rate of the target product is improved, the production cost is reduced, the generation of by-products is reduced, the commercial value of the product is improved, and the safety and environmental protection of the process are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059932A_ABST
    Figure CN119059932A_ABST
Patent Text Reader

Abstract

The present application provides a method for preparing an unsaturated nitrile, the method comprising reacting an aldehyde comprising at least one carbon-carbon double bond with a mixed gas comprising ammonia and nitrogen in a reactor containing a catalyst to produce an unsaturated nitrile comprising at least one carbon-carbon double bond, the reaction occurring in the absence of oxygen. According to the method, the synthesis of the required unsaturated nitrile can be realized by using the catalyst which is simple in composition and low in cost through simple and safe process steps, and by-products with high additional values are co-produced while the generation of substances such as toxic hydrocyanic acid and the like is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of chemical synthesis, and more specifically to a green synthesis method for preparing unsaturated nitrile. Background Art

[0002] Various unsaturated nitriles containing at least one carbon-carbon double bond and nitrile group in the molecule have extremely wide applications in the chemical industry, so people also have extremely high demand for such compounds. For example, methacrylonitrile (MAN) is a typical representative of the unsaturated nitrile, and methacrylonitrile (MAN) is an important petrochemical intermediate product. The methacrylic acid esters obtained by hydrolysis and esterification of methacrylonitrile are very important monomers, which can be used to synthesize corresponding polymers for producing materials such as coatings, inks, adhesives, plastics, rubbers, fibers, etc. In addition, methacrylonitrile itself can also be directly used as a monomer raw material to be homopolymerized or copolymerized with other monomers to form a polymer material, such as methacrylonitrile can be copolymerized with methacrylic acid to prepare polymethacrylimide (PMI) foam plastics, which is an ideal sandwich material, has the functions of low density, sound insulation, and shock absorption, and also has the characteristics of high specific strength, high specific modulus, and strong high temperature resistance, and has very good application prospects in the fields of rockets, aerospace, railways, medical treatment, and electronics. With the rapid development of related fields, people's demand for unsaturated nitriles such as methacrylonitrile (MAN) is constantly increasing.

[0003] At present, the production technologies for synthesizing unsaturated nitriles such as methacrylonitrile (MAN) mainly include ketone raw material cyanohydrin method (such as acetone cyanohydrin method), hydrocarbon raw material direct ammoxidation method (such as mixed C4 direct ammoxidation method), olefin raw material ammoxidation method (such as isobutylene ammoxidation method), and methacrylamide method. The earliest of these process routes has a development history of more than 80 years, during which it has undergone continuous process improvements. However, to date, these processes in the prior art have always had serious problems that are difficult to overcome.

[0004] For example, a serious problem with the prior art is that it inevitably produces highly toxic hydrocyanic acid by-products. This highly toxic compound can cause serious environmental pollution problems. Its storage, transportation, disposal and use are subject to strict management requirements, which increases production costs. At the same time, raw materials are also affected by the operating rate and price of upstream raw material equipment, which increases procurement costs and is not conducive to large-scale industrial production applications.

[0005] The second problem with the prior art is that its synthesis process is a highly exothermic process, and the temperature control in the process system is relatively difficult, which can easily have a serious adverse effect on the stability of the reaction, the conversion rate of raw materials and the yield of the target product, resulting in low selectivity of the target product. In addition, the mixture of ammonia and oxygen in the reaction system can easily cause a high risk of explosion.

[0006] The third problem with the prior art is that in order to obtain the desired raw material conversion rate and target product selectivity, the catalyst system has to be designed more and more complexly. In recent years, the newly developed catalysts often contain more than four and up to eight or nine metal elements. The catalysts have extremely complex element designs and microstructures. The synthesis of these catalysts will also lead to a linear increase in the overall production cost.

[0007] The fourth problem of the prior art is that a considerable proportion of the by-products produced by the process synthesis are substances that lack industrial use, have no commercial value, or are even toxic and harmful. People are eager to reduce or even eliminate these adverse by-products as much as possible. It is necessary to produce as few by-products as possible in the synthesis process, or to produce by-products with application value as much as possible.

[0008] In view of the above problems in the prior art, the inventors of the present application have conducted a lot of in-depth research and invented a novel method, which can realize the synthesis of unsaturated nitriles (such as methacrylonitrile) by a simple and low-cost process and can effectively overcome the above defects of the prior art. Summary of the invention

[0009] The present application provides a method for preparing an unsaturated nitrile, the method comprising reacting an aldehyde containing at least one carbon-carbon double bond with a mixed gas including ammonia and nitrogen in a reactor containing a catalyst to generate an unsaturated nitrile containing at least one carbon-carbon double bond, wherein the reaction occurs in the absence of oxygen.

[0010] According to one embodiment of the present application, the mixed gas also contains water vapor.

[0011] According to one embodiment of the present application, the reaction is carried out in the absence of an oxidant. According to another embodiment of the present application, the oxidant includes one or more of the following: oxygen, air, ozone, H2O2, HClO, ClO2.

[0012] According to another embodiment of the present application, the aldehyde containing at least one carbon-carbon double bond is a C3-C10 aldehyde containing at least one carbon-carbon double bond, and the unsaturated nitrile containing at least one carbon-carbon double bond is a C3-C10 nitrile containing at least one carbon-carbon double bond.

[0013] According to another embodiment of the present application, the catalyst includes a metal element supported on a carrier, and the metal element includes one or more selected from the following: copper, silver, zinc, chromium, platinum, rhodium, nickel, cobalt, molybdenum, and manganese; the carrier includes one or more of the following: aluminum oxide, silicon oxide, and magnesium aluminate.

[0014] According to another embodiment of the present application, based on the total weight of the catalyst, the content of the metal element is 0.1 wt % to 60 wt %.

[0015] According to another embodiment of the present application, the metal element includes one or more selected from the following: silver, platinum, rhodium, chromium, and the content of the metal element is 1 wt% to 4 wt% based on the total weight of the catalyst. According to another embodiment of the present application, the metal element includes one or more selected from the following: copper, zinc, chromium, nickel, cobalt, molybdenum, manganese, and the content of the metal element is 20 wt% to 36 wt% based on the total weight of the catalyst.

[0016] According to another embodiment of the present application, the reaction is carried out at a reaction temperature of 250-450°C and a reaction pressure of 1 to 5 atmospheres. According to another embodiment of the present application, the particle size of the catalyst is 10-60 mesh, and before the reaction, the catalyst is pretreated with a mixed gas containing H2 at a pretreatment temperature of 300-500°C.

[0017] According to another embodiment of the present application, the reaction is carried out in a continuous manner, and the aldehyde containing at least one carbon-carbon double bond is heated at a rate of 0.1-1.6 hours. -1 The space velocity is supplied to the reaction.

[0018] According to another embodiment of the present application, the volume ratio of the aldehyde containing at least one carbon-carbon double bond and ammonia input into the reactor is 1:0.8 to 1:10. According to another embodiment of the present application, the volume ratio of the aldehyde containing at least one carbon-carbon double bond and nitrogen input into the reactor is 1:0.9 to 1:10.5. According to another embodiment of the present application, in the case where the mixed gas contains water vapor, the volume ratio of the aldehyde containing at least one carbon-carbon double bond and water vapor input into the reactor is 1:1 to 1:5.

[0019] According to another embodiment of the present application, the reaction does not generate hydrocyanic acid.

[0020] In the specific implementation section below, the method and prepared product of the present application are further introduced in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1A and Figure 1B A reaction device for preparing methacrylonitrile according to one embodiment of the present application is shown;

[0022] Figure 2 A gas chromatography device for detecting the content of reaction products and by-products according to one embodiment of the present application is shown;

[0023] Figure 3 The catalysts synthesized in some examples of the present application are shown;

[0024] Figure 4A and 4B A gas chromatographic curve diagram of the detection product n-butanol absorption liquid and tail gas according to one embodiment of the present application is shown. DETAILED DESCRIPTION

[0025] "Range" disclosed herein is in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges that can be defined in this way are inclusive and combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.

[0026] In this application, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations.

[0027] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.

[0028] In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.

[0029] In this application, if there is no special explanation, the "including" mentioned herein means open or closed. For example, the "including" may mean that other components not listed may also be included, or only the listed components may be included.

[0030] The method of the present invention comprises reacting an aldehyde containing at least one carbon-carbon double bond (hereinafter also referred to as "unsaturated aldehyde") with a mixed gas including ammonia and nitrogen in a reactor containing a catalyst to generate an unsaturated nitrile containing at least one carbon-carbon double bond, wherein the reaction occurs in the absence of oxygen.

[0031] According to one embodiment of the present application, the mixed gas contains water vapor in addition to ammonia and nitrogen. According to another independent embodiment of the present application, the mixed gas contains only ammonia and nitrogen but no water vapor.

[0032] The first aspect of the present invention is that the above reaction is carried out in the absence of oxygen. In the present invention, the so-called "absence of oxygen" means that no oxygen-containing stream (such as pure oxygen stream, air stream, etc.) is intentionally input into the reactor, and the above oxygen-containing substances are avoided as much as possible in the various reaction raw materials during the reaction.

[0033] According to another embodiment of the present application, during the entire process of the reaction of the present invention, no oxidant is intentionally introduced into the reactor, and substances containing oxidants are avoided as much as possible in various reaction raw materials during the reaction. In the present invention, examples of the oxidants that are avoided as much as possible in the reaction of the present invention include, but are not limited to, oxygen, air, ozone, H2O2, HClO, ClO2, etc.

[0034] For example, the purpose of avoiding the introduction of oxygen or other oxidants can be achieved by replacing the atmosphere in the reactor with a reducing or inert gas before the reaction, and / or detecting oxygen or any other oxidants that may be mixed in the raw materials (such as unsaturated aldehydes, water vapor, ammonia, nitrogen) input into the reactor, and purifying these raw materials when necessary to remove the mixed oxygen or any other oxidants.

[0035] According to an exemplary embodiment of the present application, during the reaction of the present invention, only unsaturated aldehyde, water vapor, ammonia and nitrogen are input into the reactor, and no other components are input. According to another independent exemplary embodiment of the present application, during the reaction of the present invention, only unsaturated aldehyde, ammonia and nitrogen are input into the reactor, and no other components are input. It should be noted that the solid catalyst pre-loaded in the reactor and the atmosphere used for the pretreatment catalyst (e.g., hydrogen / nitrogen mixed gas) will not affect the operation of "no other components will be input during the reaction" described above.

[0036] According to one embodiment of the present application, the molecule of the aldehyde comprising at least one carbon-carbon double bond comprises 1-4 carbon-carbon double bonds, such as 1-2 carbon-carbon double bonds, preferably comprises one carbon-carbon double bond. According to another embodiment of the present application, the aldehyde (unsaturated aldehyde) comprising at least one carbon-carbon double bond is a C3-C10 unsaturated aldehyde, such as a C3-C6 unsaturated aldehyde, preferably methacrolein or acrolein. Accordingly, the unsaturated nitrile (hereinafter also referred to as "unsaturated nitrile") containing at least one carbon-carbon double bond synthesized by the inventive method is a C3-C10 nitrile containing at least one carbon-carbon double bond, such as a C3-C6 unsaturated nitrile, preferably methacrolein or acrylonitrile.

[0037] In the following text, some specific embodiments of the present application are discussed and illustrated mainly by taking “methacrolein reacts with water vapor, ammonia and nitrogen to generate the target product methacrylonitrile” or “methacrolein reacts with ammonia and nitrogen to generate the target product methacrylonitrile” as an example, but the scope of the present application is not limited to this.

[0038] According to one embodiment of the application, the reaction can be carried out in a continuous manner. For example, the unsaturated aldehyde, ammonia, nitrogen and water vapor (if water vapor is used) can be continuously input into the reactor, react under the condition of contacting (contacting at the gas-solid phase interface) with the solid catalyst pre-filled in the reactor, generate the target product unsaturated nitrile, and then make the reacted material be continuously exported from the reactor under the driving effect of the fresh material of the subsequent input. According to one embodiment of the application, the above-mentioned unsaturated aldehyde, ammonia, nitrogen and water vapor (if water vapor is used) logistics can be independently input into the reactor, and any two or more logistics can be pre-mixed, and then input into the reactor. According to one embodiment of the application, the reactor includes a fixed bed reactor or a fluidized bed reactor, such as a tubular fixed bed reactor.

[0039] According to one embodiment of the present application, the unsaturated aldehyde as a raw material is liquid at normal temperature and pressure. It is first input into a preheating device, and the preheating device has a temperature higher than the boiling point of the unsaturated aldehyde. For example, the preheater temperature can be 200-250°C. The liquid unsaturated aldehyde is preheated in the preheater to convert the unsaturated aldehyde from a liquid phase to a gas phase. Subsequently, the gaseous unsaturated aldehyde is transported to a reactor to react with ammonia, nitrogen and water vapor (if water vapor is used) which are also in a gaseous state.

[0040] According to one embodiment of the present application, the unsaturated aldehyde flow rate is 0.1-1.6 hours. -1 The space velocity is provided to the reaction, for example, the space velocity can be 0.13-1.6 hours -1 , or 0.4-1.2 hours-1 , or 0.6-1.0 hours -1 , or 0.8-0.9 hours -1 It should be emphasized here that the "space velocity of the unsaturated aldehyde flow" mentioned here refers to the space velocity of the unsaturated aldehyde flow alone, and has nothing to do with other substances (such as ammonia, nitrogen, water vapor, etc.) provided to the reaction.

[0041] According to one embodiment of the present application, the flow rates of various reaction materials (more specifically, gas flow rates) input during the reaction process conform to a specific designed ratio.

[0042] According to an exemplary embodiment, the volume ratio (gas flow ratio) of the unsaturated aldehyde to ammonia input into the reactor is 1:0.8 to 1:10, for example 1:1 to 1:8, or 1:1 to 1:7.5, or 1:2.5 to 1:5, or 1:2.5 to 1:7.5, or 1:5 to 1:7.5.

[0043] According to another exemplary embodiment, the volume ratio of the unsaturated aldehyde to nitrogen (gas flow ratio) input into the reactor is 1:0.9 to 1:10.5, for example 1:1 to 1:10, or 1:1 to 1:5.5, or 1:1 to 1:5, or 1:2.5 to 1:5.

[0044] According to another exemplary embodiment, no water vapor is input into the reactor, in which case the flow rate of the water vapor is zero.

[0045] According to another exemplary embodiment, when the reaction includes water vapor, the volume ratio (gas flow ratio) of the unsaturated aldehyde to water vapor input into the reactor is 1:1 to 1:5, for example, 1:1 to 1:2.5, or 1:2.5 to 1:5.

[0046] According to one embodiment of the present application, the reaction temperature is 250-450° C., such as 290-410° C., or 290-320° C., or 340-360° C., or 290-410° C. According to another embodiment of the present application, the reaction is carried out under 1-5 atmospheres, such as 1-3 atmospheres, preferably at normal pressure.

[0047] The second inventive point of the present invention is to achieve improvements in raw material conversion rate and target product selectivity by optimizing the design of the above process conditions.

[0048] The third inventive point of the present invention is that the catalyst used in the present invention has an extremely simple composition design. The use of this simple catalyst can achieve excellent raw material conversion rate and target product selectivity, avoid the formation of toxic and harmful hydrocyanic acid by-products, and avoid the increase in cost and process complexity caused by complex catalyst composition design.

[0049] According to one embodiment of the present application, the catalyst includes a metal element supported on a carrier, and the metal element includes one or more selected from the following: copper, silver, zinc, chromium, platinum, rhodium, nickel, cobalt, molybdenum, and manganese; the carrier includes one or more of the following: aluminum oxide, silicon oxide, and magnesium aluminate.

[0050] According to one embodiment of the present application, the metal element includes one or more selected from the following, preferably one or two selected from the following: silver, platinum, rhodium, and the content of the metal element is 1 wt% to 4 wt%, such as 1.5-3.5 wt%, or 1.8-3.3 wt%, based on the total weight of the catalyst. According to another embodiment of the present application, the metal element includes one or more selected from the following, preferably one or two selected from the following: copper, zinc, chromium, nickel, cobalt, molybdenum, manganese, and the content of the metal element is 20 wt% to 36 wt%, based on the total weight of the catalyst.

[0051] According to an exemplary embodiment of the present application, the metal element is copper, and based on the total weight of the catalyst, the content of copper is 25 wt % to 35 wt %, preferably 30-34 wt %.

[0052] According to another exemplary embodiment of the present application, the metal element is molybdenum, and the content of the molybdenum is 22 wt % to 30 wt %, preferably 24-28 wt %, based on the total weight of the catalyst.

[0053] According to another exemplary embodiment of the present application, the metal element is nickel, and the content of the nickel is 24 wt % to 32 wt %, preferably 26-29 wt %, based on the total weight of the catalyst.

[0054] According to another exemplary embodiment of the present application, the metal element is a mixture of copper and chromium, and based on the total weight of the catalyst, the copper content is 15 wt % to 26 wt %, preferably 18-22 wt %; the chromium content is 1.5 wt % to 6 wt %, preferably 2-3 wt %.

[0055] According to another exemplary embodiment of the present application, the metal element is platinum, and based on the total weight of the catalyst, the content of the platinum is 1.2 wt% to 3.8 wt%, preferably 2-3.6 wt%, and more preferably 2.5-3.5 wt%.

[0056] According to another exemplary embodiment of the present application, the metal element is silver, and based on the total weight of the catalyst, the content of the silver is 1 wt % to 3.5 wt %, preferably 1.2-3 wt %, more preferably 1.5-2 wt %.

[0057] According to one embodiment, the catalyst of the present application is prepared by the following method: a solution (e.g., an aqueous solution) is prepared using a metal soluble salt, the solution of the metal salt is fully mixed with a solid carrier, the mixture is allowed to stand for a period of time, for example, 1-24 hours, or 12-24 hours, so that the metal salt solution is fully adsorbed into the carrier, and then the mixture is heated, dried, and calcined to obtain the catalyst of the present invention.

[0058] According to one embodiment, after the calcination, the solid material obtained by calcination can be ground, tableted and sieved, so that the obtained catalyst has a particle size within a specific range, such as 10-60 mesh.

[0059] According to one embodiment of the present application, the catalyst needs to be pretreated before being used in the reaction. Specifically, after the desired catalyst is loaded into the reactor, the catalyst is first pretreated with a reducing gas, and the reducing gas can be hydrogen or a mixture of hydrogen and nitrogen. For the case of a mixture of hydrogen and nitrogen, the mixed volume ratio of hydrogen and nitrogen can be 50:50 to 90:10, for example, 70:30 to 80:20. According to one embodiment of the present application, the pretreatment temperature can be 200-500°C, for example, 250-400°C, or 300-350°C. The pretreatment time can be 0.5-12 hours, for example, 0.8-6 hours, or 1-3 hours.

[0060] According to one embodiment of the present application, due to the above-mentioned pretreatment, before the reaction begins, a portion of the metal elements in the catalyst of the present invention are reduced to zero valence, for example, more than 30%, more than 50%, more than 60%, more than 70% are reduced to zero valence, or more than 90% are reduced to zero valence, or all are reduced to zero valence. The valence state of the metal elements in the catalyst is related to the above-mentioned pretreatment conditions, as well as the type of metal elements, the content of metal elements, the microscopic morphology of the carrier and the distribution of the metal elements in the carrier. The present application does not strictly require the valence state of the metal elements in the catalyst.

[0061] According to one embodiment of the present application, the product synthesized by the method of the present application contains no toxic hydrocyanic acid byproducts at all, specifically, contains no detectable hydrocyanic acid byproducts.

[0062] According to another embodiment of the present application, most of the mixed by-products in the product obtained by the synthesis method of the present application (for example, greater than 50 mol%, or greater than 70 mol%, or greater than 80 mol%, or greater than 90%, or greater than 95 mol%, based on the total molar amount of all by-products) are compounds with application prospects and commercial value. For example, in the reaction of preparing methacrylonitrile from methacrolein, the synthesized product mainly contains the target product methacrylonitrile, and the by-products are mainly isobutyronitrile and 3,5-lutidine, both of which have high market value.

[0063] The method of the present invention can achieve the following advantages:

[0064] (1) Improved production efficiency: The method of the present invention is carried out in a continuous manner and can complete the reaction process in a shorter time, thereby greatly improving production efficiency.

[0065] (2) Improving product quality: The method of the present invention can effectively improve the yield of unsaturated nitrile (such as methacrylonitrile), reduce the generation of toxic and harmful by-products, reduce the types of by-products, and the by-products have high economic value.

[0066] (3) Environmental protection: In the method of the present invention, the generation of toxic and harmful substances such as hydrocyanic acid can be effectively avoided, thereby reducing the risk of environmental pollution and the cost of post-processing.

[0067] (4) High safety of the operation process: In the method of the present invention, no strong oxidants such as oxygen are involved in the reaction throughout the process, which can effectively avoid the risk of equipment explosion during the reaction.

[0068] (5) Good market economics: By optimizing the reaction conditions and catalyst design, higher raw material conversion rates and product selectivity can be achieved, achieving excellent market value.

[0069] (6) Easy to scale up production: The method of the present invention is sophisticated in design, simple in operation, and low in cost. It can be easily industrialized and further scaled up based on existing equipment.

[0070] In the following examples, the method of the present application is specifically described with specific examples, and its purpose is to better understand the content of the present application. It should be understood that these examples are merely illustrative and non-restrictive. The reagents used in the examples are conventionally purchased from the market unless otherwise specified. The methods and conditions used in the examples are conventional methods and conditions unless otherwise specified.

[0071] Example

[0072] All reagents used in the following examples were of analytical grade, so the water used was deionized water. Figure 2 The product absorption liquid was characterized by a Trace 1310 gas chromatograph (equipped with a WAX column) produced by Thermo Fisher Scientific, and the tail gas was characterized by a Thermo Fisher Scientific ISQ7000 gas chromatography-mass spectrometry (GC-MS) instrument (equipped with an HP column).

[0073] In addition, in the following examples, the raw material conversion rate and product selectivity of various components were calculated according to the following formula:

[0074] Methacrolein conversion rate = (1-methacrolein mole fraction in reaction product / methacrolein mole fraction in feed) × 100%;

[0075] Methacrylonitrile selectivity = mole fraction of methacrylonitrile in the reaction product / (mole fraction of methacrolein in the feed - mole fraction of methacrolein in the reaction product) × 100%;

[0076] Isobutyronitrile selectivity = isobutyronitrile mole fraction in the reaction product / (methacrolein mole fraction in the feed - methacrolein mole fraction in the reaction product) × 100%;

[0077] 3,5-Lutidine selectivity = 3,5-Lutidine mole fraction in the reaction product / (methacrolein mole fraction in the feed - methacrolein mole fraction in the reaction product) × 100%;

[0078] Hydrocyanic acid selectivity = mole fraction of hydrocyanic acid in the reaction product / (mole fraction of methacrolein in the feed - mole fraction of methacrolein in the reaction product) × 100%.

[0079] Example 1

[0080] In this example, firstly, an aluminum oxide-supported copper (Cu / Al2O3) catalyst was synthesized in the following manner.

[0081] Weigh 100 grams of solid copper nitrate (Cu(NO3)2·3H2O) and place it in a beaker. Add deionized water to the beaker at room temperature and stir until the solid is completely dissolved to form a solution with a Cu content of 32% by weight. Mix the above solution with 50 grams of aluminum oxide powder and stir evenly. Then, place the suspension at room temperature for 24 hours, and then place it in an oven at 120°C for 12 hours to completely dry the suspension. Grind the dried solid, put it in a muffle furnace, heat it to 550°C at a heating rate of 2°C / min in an air atmosphere, and calcine it at this temperature for 12 hours. The calcined solid is ground, tableted, and sieved to obtain a Cu / Al2O3 catalyst with a particle size of 10-20 mesh. The Cu content is measured to be 33.1% by weight using the Optima 7000DV plasma emission spectrometer (ICP) of PE Company of the United States. The catalyst synthesized in this way is as follows Figure 3 shown.

[0082] Next in Figure 1A and Figure 1B In the reaction system shown in FIG. 1 , a catalytic reaction is carried out using the catalyst prepared in the above steps. Figure 1A As shown, the reaction system includes a preheater, a reactor and an absorption device in sequence, such as Figure 1B As shown, the process parameters of the reaction system are controlled by a control panel. Specifically, 4 g of catalyst is weighed and loaded into a tubular reactor ( Figure 1A The tubular reactor is shown to have a constant temperature zone (temperature control device) outside. A mixed gas of 80% H2 / 20% N2 is introduced into the reactor at a flow rate of 100 ml / min, and the catalyst is pretreated at a temperature of 300°C for 1 hour.

[0083] Liquid methacrolein is fed into a preheater at 240° C. to convert it from liquid to gas. Methacrolein, ammonia, nitrogen and water vapor are mixed in the preheater at a volume ratio of 1:5:1:1. The mixture is then continuously fed into the tubular reactor. The reactor temperature is maintained at about 300° C., the pressure is normal pressure, and the space velocity of methacrolein is 0.8 h / min. -1 .

[0084] The gaseous product flow from the reactor enters the condensing coil. After the reaction has been carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Figure 2 The gas chromatography was characterized by comparing the gas chromatography with the standard sample to perform qualitative analysis, and the standard curve was used for quantitative calculation to obtain the raw material conversion rate and the selectivity of different main and by-products. Figure 4AThe gas chromatogram of the absorption liquid is shown. The test results are summarized in Table 1.

[0085] The tail gas after absorption by n-butanol was directly sampled for GC-MS testing. Figure 4B The gas chromatogram of the tail gas is shown, indicating that it is mainly n-butanol (absorbent liquid) and contains substantially no organic byproducts, especially no hydrocyanic acid. The tail gas is treated with water and sulfuric acid solution in sequence and then discharged into the atmosphere.

[0086] Example 2

[0087] In this example, the synthesis of a silica-supported molybdenum (Mo / SiO2) catalyst was first performed in the same manner as in Example 1, except that 36.8 g of ammonium molybdate ((NH4)6Mo7O 24 ·4H2O) to prepare a 25 wt% aqueous solution, which was then mixed with 50 g of silicon dioxide. The final molybdenum content in the catalyst was 25.6 wt%. The catalyst thus synthesized was Figure 3 shown.

[0088] Next, the catalytic reaction was carried out using the catalyst prepared in the above steps using the same reaction system as in Example 1. Specifically, 4 g of the catalyst was weighed and loaded into the constant temperature zone of a tubular reactor made of 316L stainless steel and having an inner diameter of 8 mm. A mixed gas of 80% H2 / 20% N2 was introduced into the reactor at a flow rate of 200 ml / min, and the catalyst was pretreated at a temperature of 500°C for 1 hour.

[0089] Liquid methacrolein is fed into a preheater at 240°C to convert it from liquid to gas. Methacrolein, ammonia, nitrogen and water vapor are mixed in the preheater at a volume ratio of 1:1:5:1. The mixture is then continuously fed into the tubular reactor. The reactor temperature is maintained at about 350°C, the pressure is normal pressure, and the space velocity of methacrolein is 0.8 hours. -1 .

[0090] The gaseous product flow from the reactor enters the condensing coil. After the reaction is carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using a n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Qualitative analysis is performed by comparing gas chromatography with the standard sample, and quantitative calculation is performed by the standard curve to obtain the raw material conversion rate and the selectivity of different main and by-products. The test results are summarized in Table 1.

[0091] The tail gas after liquid absorption is sampled and tested by GC-MS to determine that it is mainly n-butanol (absorption liquid) and substantially free of organic byproducts, especially hydrocyanic acid. The tail gas is treated with water and sulfuric acid solution in sequence and then discharged into the atmosphere.

[0092] Example 3

[0093] In this example, the Ni / MgAl2O4 catalyst was first synthesized in the same manner as in Example 1, except that 120 g of nickel nitrate (Ni(NO3)2·6H2O) was used to prepare a 30 wt% aqueous solution, which was then mixed with 50 g of MgAl2O4, resulting in a nickel content of 28.3 wt% in the catalyst. The catalyst thus synthesized was Figure 3 shown.

[0094] Next, the catalytic reaction was carried out using the catalyst prepared in the above steps in the same reaction system as in Example 1. Specifically, 4 g of the catalyst was weighed and loaded into the constant temperature zone of a tubular reactor made of 316L stainless steel and having an inner diameter of 8 mm. A mixed gas of 80% H2 / 20% N2 was introduced into the reactor at a flow rate of 100 ml / min, and the catalyst was pretreated at a temperature of 450°C for 1 hour.

[0095] Liquid methacrolein is fed into a preheater at 240° C. to be converted from liquid to gaseous state. Methacrolein, ammonia, nitrogen and water vapor are mixed in the preheater at a volume ratio of 1:2.5:2.5:1. The mixture is then continuously fed into the tubular reactor. The temperature of the reactor is maintained at about 300° C., the pressure is normal pressure, and the space velocity of methacrolein is 0.8 h / min. -1 .

[0096] The gaseous product flow from the reactor enters the condensing coil. After the reaction is carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using a n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Qualitative analysis is performed by comparing gas chromatography with the standard sample, and quantitative calculation is performed by the standard curve to obtain the raw material conversion rate and the selectivity of different main and by-products. The test results are summarized in Table 1.

[0097] The tail gas after liquid absorption is sampled and tested by GC-MS to determine that it is mainly n-butanol (absorption liquid) and substantially free of organic byproducts, especially hydrocyanic acid. The tail gas is treated with water and sulfuric acid solution in sequence and then discharged into the atmosphere.

[0098] Example 4

[0099] In this example, the Pt / Al2O3 catalyst was first synthesized in the same manner as in Example 1, except that 4.2 g of chloroplatinic acid (H2PtCl6·6H2O) was used to prepare a 3 wt% aqueous solution, which was then mixed with 50 g of Al2O3, resulting in a final catalyst having a platinum content of 3.3 wt%. The catalyst thus synthesized was Figure 3 shown.

[0100] Next, the catalytic reaction was carried out using the catalyst prepared in the above steps in the same reaction system as in Example 1. Specifically, 4 g of the catalyst was weighed and loaded into the constant temperature zone of a tubular reactor made of 316L stainless steel and having an inner diameter of 8 mm. A mixed gas of 50% H2 / 50% N2 was introduced into the reactor at a flow rate of 200 ml / min, and the catalyst was pretreated at a temperature of 450°C for 1 hour.

[0101] Liquid methacrolein is fed into a preheater at 240°C to convert it from liquid to gas. Methacrolein, ammonia, nitrogen and water vapor are mixed in a volume ratio of 1:2.5:5:1 in the preheater. The mixture is then continuously fed into the tubular reactor. The temperature of the reactor is maintained at about 350°C, the pressure is normal pressure, and the space velocity of methacrolein is 0.8 hours. -1 .

[0102] The gaseous product flow from the reactor enters the condensing coil. After the reaction is carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using a n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Qualitative analysis is performed by comparing gas chromatography with the standard sample, and quantitative calculation is performed by the standard curve to obtain the raw material conversion rate and the selectivity of different main and by-products. The test results are summarized in Table 1.

[0103] The tail gas after liquid absorption is sampled and tested by GC-MS to determine that it is mainly n-butanol (absorption liquid) and substantially free of organic byproducts, especially hydrocyanic acid. The tail gas is treated with water and sulfuric acid solution in sequence and then discharged into the atmosphere.

[0104] Example 5

[0105] In this example, the Ag / SiO2 catalyst was first synthesized in the same manner as in Example 1, except that 1.6 g of silver nitrate (AgNO3) was used to prepare an aqueous solution with a concentration of 2 wt%, and then the aqueous solution was mixed with 50 g of SiO2, and the silver content in the final catalyst was 1.8 wt%. The catalyst synthesized in this way is as follows Figure 3 shown.

[0106] Next, the catalytic reaction was carried out using the catalyst prepared in the above steps using the same reaction system as in Example 1. Specifically, 4 g of the catalyst was weighed and loaded into the constant temperature zone of a tubular reactor made of 316L stainless steel and having an inner diameter of 8 mm. A mixed gas of 60% H2 / 40% N2 was introduced into the reactor at a flow rate of 150 ml / min, and the catalyst was pretreated at a temperature of 400°C for 1 hour.

[0107] Liquid methacrolein is input into a preheater at 240° C. to convert it from liquid to gaseous state. Methacrolein, ammonia, nitrogen and water vapor are mixed in the preheater at a volume ratio of 1:5:5:2.5. The mixture is then continuously input into the tubular reactor. The temperature of the reactor is maintained at about 400° C., the pressure is normal pressure, and the space velocity of methacrolein is 0.8 h / min. -1 .

[0108] The gaseous product flow from the reactor enters the condensing coil. After the reaction is carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using a n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Qualitative analysis is performed by comparing gas chromatography with the standard sample, and quantitative calculation is performed by the standard curve to obtain the raw material conversion rate and the selectivity of different main and by-products. The test results are summarized in Table 1.

[0109] The tail gas after liquid absorption is sampled and tested by GC-MS to determine that it is mainly n-butanol (absorption liquid) and substantially free of organic byproducts, especially hydrocyanic acid. The tail gas is treated with water and sulfuric acid solution in sequence and then discharged into the atmosphere.

[0110] Example 6

[0111] In this example, the Cu-Cr / Al2O3 catalyst was first synthesized in the same manner as in Example 1, except that 52.5 g of copper nitrate (Cu(NO3)2·3H2O), 10.8 g of chromium nitrate (Cr(NO3)3·9H2O) and 50 ml of water were used to prepare an aqueous solution, which was then mixed with 50 g of Al2O3. The final catalyst had a copper content of 20.6% by weight and a chromium content of 2.3% by weight. The catalyst thus synthesized was Figure 3 shown.

[0112] Next, the catalytic reaction was carried out using the catalyst prepared in the above steps using the same reaction system as in Example 1. Specifically, 4 g of the catalyst was weighed and loaded into the constant temperature zone of a tubular reactor made of 316L stainless steel and having an inner diameter of 8 mm. A mixed gas of 80% H2 / 20% N2 was introduced into the reactor at a flow rate of 100 ml / min, and the catalyst was pretreated at a temperature of 350°C for 1 hour.

[0113] Liquid methacrolein is fed into a preheater at 240° C. to convert it from liquid to gaseous state. Methacrolein, ammonia, nitrogen and water vapor are mixed in the preheater at a volume ratio of 1:7.5:5:5. The mixture is then continuously fed into the tubular reactor. The temperature of the reactor is maintained at about 300° C., the pressure is normal pressure, and the space velocity of methacrolein is 0.8 h / min. -1 .

[0114] The gaseous product flow from the reactor enters the condensing coil. After the reaction is carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using a n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Qualitative analysis is performed by comparing gas chromatography with the standard sample, and quantitative calculation is performed by the standard curve to obtain the raw material conversion rate and the selectivity of different main and by-products. The test results are summarized in Table 1.

[0115] The tail gas after liquid absorption is sampled and tested by GC-MS to determine that it is mainly n-butanol (absorption liquid) and substantially free of organic byproducts, especially hydrocyanic acid. The tail gas is treated with water and sulfuric acid solution in sequence and then discharged into the atmosphere.

[0116] Example 7

[0117] In this Example 7, the reaction was carried out without using water vapor.

[0118] Specifically, using the same reaction system as in Example 1, 4 g of the catalyst synthesized in Example 3 was weighed and loaded into the constant temperature zone of a tubular reactor made of 316L stainless steel and having an inner diameter of 8 mm. A mixed gas of 80% H2 / 20% N2 was introduced into the reactor at a flow rate of 100 ml / min, and the catalyst was pretreated at a temperature of 450°C for 1 hour.

[0119] Liquid methacrolein is input into a preheater at 240° C. to convert it from liquid to gas. Methacrolein, ammonia and nitrogen are mixed in the preheater at a volume ratio of 1:5:2.5, and then the mixture is continuously input into the tubular reactor. The temperature of the reactor is maintained at about 300° C., the pressure is normal pressure, and the space velocity of methacrolein is 0.8 h / min. -1 .

[0120] The gaseous product flow from the reactor enters the condensing coil. After the reaction is carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using a n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Qualitative analysis is performed by comparing gas chromatography with the standard sample, and quantitative calculation is performed by the standard curve to obtain the raw material conversion rate and the selectivity of different main and by-products. The test results are summarized in Table 1.

[0121] The tail gas after liquid absorption is sampled and tested by GC-MS to determine that it is mainly n-butanol (absorption liquid) and substantially free of organic byproducts, especially hydrocyanic acid. The tail gas is treated with water and sulfuric acid solution in sequence and then discharged into the atmosphere.

[0122] Comparative Example 1

[0123] In this comparative example 1, the catalyst described in the above example 1 was used and the reaction was carried out in a reaction system containing oxygen (air).

[0124] Specifically, using the same reaction system as in Example 1, 4 g of the catalyst synthesized in Example 1 was weighed and loaded into the constant temperature zone of a tubular reactor made of 316L stainless steel and having an inner diameter of 8 mm. A mixed gas of 80% H2 / 20% N2 was introduced into the reactor at a flow rate of 100 ml / min, and the catalyst was pretreated at a temperature of 300°C for 1 hour.

[0125] Liquid methacrolein is input into a preheater at 240° C. to convert it from liquid to gas. Methacrolein, ammonia, nitrogen, water vapor and air are mixed in the preheater at a volume ratio of 1:5:1:1:1. The mixture is then continuously input into the tubular reactor. The temperature of the reactor is maintained at about 300° C., the pressure is normal pressure, and the space velocity of methacrolein is 0.8 h / min. -1 .

[0126] The gaseous product flow from the reactor enters the condensing coil. After the reaction is carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using a n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Qualitative analysis is performed by comparing gas chromatography with the standard sample, and quantitative calculation is performed by the standard curve to obtain the raw material conversion rate and the selectivity of different main and by-products. The test results are summarized in Table 1.

[0127] The tail gas after liquid absorption is treated with water phase, sulfuric acid solution and sodium hydroxide solution in sequence to fully remove the by-products (especially hydrocyanic acid) contained therein, and then discharged into the atmosphere.

[0128] Comparative Example 2

[0129] In this comparative example 2, the catalyst described in the above example 2 was used and the reaction was carried out in a reaction system containing oxygen (air).

[0130] Specifically, using the same reaction system as in Example 1, 4 g of the catalyst synthesized in Example 2 was weighed and loaded into the constant temperature zone of a tubular reactor made of 316L stainless steel and having an inner diameter of 8 mm. A mixed gas of 80% H2 / 20% N2 was introduced into the reactor at a flow rate of 200 ml / min, and the catalyst was pretreated at a temperature of 500°C for 1 hour.

[0131] Liquid methacrolein is fed into a preheater at 240° C. to convert it from liquid to gaseous state. Methacrolein, ammonia, nitrogen, water vapor and air are mixed in the preheater at a volume ratio of 1:1:5:1:1. The mixture is then continuously fed into the tubular reactor. The temperature of the reactor is maintained at about 350° C., the pressure is normal pressure, and the space velocity of methacrolein is 0.8 h / min. -1 .

[0132] The gaseous product flow from the reactor enters the condensing coil. After the reaction is carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using a n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Qualitative analysis is performed by comparing gas chromatography with the standard sample, and quantitative calculation is performed by the standard curve to obtain the raw material conversion rate and the selectivity of different main and by-products. The test results are summarized in Table 1.

[0133] The tail gas after liquid absorption is treated with water phase, sulfuric acid solution and sodium hydroxide solution in sequence to fully remove the by-products (especially hydrocyanic acid) contained therein, and then discharged into the atmosphere.

[0134] Comparative Example 3

[0135] In this comparative example 3, the catalyst described in the above example 3 was used and the reaction was carried out in a reaction system containing oxygen (air).

[0136] Specifically, using the same reaction system as in Example 1, 4 g of the catalyst synthesized in Example 3 was weighed and loaded into the constant temperature zone of a tubular reactor made of 316L stainless steel and having an inner diameter of 8 mm. A mixed gas of 80% H2 / 20% N2 was introduced into the reactor at a flow rate of 100 ml / min, and the catalyst was pretreated at a temperature of 450°C for 1 hour.

[0137] Liquid methacrolein is fed into a preheater at 240° C. to convert it from liquid to gaseous state. Methacrolein, ammonia, nitrogen, water vapor and air are mixed in the preheater at a volume ratio of 1:2.5:2.5:1:1. The mixture is then continuously fed into the tubular reactor. The temperature of the reactor is maintained at about 300° C., the pressure is normal pressure, and the space velocity of methacrolein is 0.8 h / min. -1 .

[0138] The gaseous product flow from the reactor enters the condensing coil. After the reaction is carried out for 3 hours and has stabilized, the gaseous product is absorbed for 10 minutes using a n-butanol solution to obtain a liquid absorption liquid, to which 0.1 g of cyclohexanone is added as an internal standard. Qualitative analysis is performed by comparing gas chromatography with the standard sample, and quantitative calculation is performed by the standard curve to obtain the raw material conversion rate and the selectivity of different main and by-products. The test results are summarized in Table 1.

[0139] The tail gas after liquid absorption is treated with water phase, sulfuric acid solution and sodium hydroxide solution in sequence to fully remove the by-products (especially hydrocyanic acid) contained therein, and then discharged into the atmosphere.

[0140] It can be seen from the experimental data in Table 1 that, compared with Comparative Examples 1-3 (which use a reaction process containing oxygen, corresponding to the prior art), Examples 1-7 of the present invention completely avoid the generation of toxic hydrocyanic acid byproducts, and achieve a raw material aldehyde conversion rate that is not inferior to the prior art, and the yield of the target product methacrylonitrile is significantly improved. In addition, the proportion of products with high commercial value in the products synthesized by the present invention is also significantly increased.

[0141] Table 1: Aldehyde conversion and product selectivity of Examples 1-7 and Comparative Examples 1-3

[0142]

[0143] In addition, through the optimization design of the process, Examples 1-2 and Example 6 can achieve a better ratio of valuable products, among which Example 6 obtains the best result.

Claims

1. A method for preparing an unsaturated nitrile, the method comprising reacting an aldehyde comprising at least one carbon-carbon double bond with a mixed gas comprising ammonia and nitrogen in a reactor containing a catalyst to generate an unsaturated nitrile comprising at least one carbon-carbon double bond, the reaction occurring in the absence of oxygen.

2. The method according to claim 1, characterized in that The mixed gas also contains water vapor.

3. The method according to claim 1, characterized in that The reaction is carried out in the absence of an oxidant, which includes one or more of the following: oxygen, air, ozone, H2O2, HClO, ClO2.

4. The method according to claim 1, characterized in that The aldehyde containing at least one carbon-carbon double bond is a C3-C10 aldehyde containing at least one carbon-carbon double bond, and the unsaturated nitrile containing at least one carbon-carbon double bond is a C3-C10 nitrile containing at least one carbon-carbon double bond.

5. The method according to claim 1, characterized in that The catalyst includes a metal element supported on a carrier, and the metal element includes one or more selected from the following: copper, silver, zinc, chromium, platinum, rhodium, nickel, cobalt, molybdenum, and manganese; the carrier includes one or more of the following: aluminum oxide, silicon oxide, and magnesium aluminate; based on the total weight of the catalyst, the content of the metal element is 0.1 weight % to 60 weight %.

6. The method according to claim 5, characterized in that The metal element comprises one or more selected from the following: silver, platinum, rhodium, and the content of the metal element is 1 wt % to 4 wt % based on the total weight of the catalyst; or The metal elements include one or more selected from the following: copper, zinc, chromium, nickel, cobalt, molybdenum, and manganese, and the content of the metal elements is 20 wt % to 36 wt % based on the total weight of the catalyst.

7. The method according to claim 1, characterized in that The reaction is carried out at a reaction temperature of 250-450° C. and a reaction pressure of 1 to 5 atmospheres; The particle size of the catalyst is 10-60 meshes. Before the reaction, the catalyst is pretreated with a mixed gas containing H2 at a pretreatment temperature of 300-500°C.

8. The method according to claim 1, characterized in that The reaction is carried out in a continuous manner and the aldehyde containing at least one carbon-carbon double bond is heated at a rate of 0.1 to 1.6 hours. -1 The space velocity is supplied to the reaction.

9. The method according to any one of claims 1 to 8, characterized in that The volume ratio of the aldehyde containing at least one carbon-carbon double bond to ammonia input into the reactor is 1:0.8 to 1:10; The volume ratio of the aldehyde containing at least one carbon-carbon double bond to nitrogen input into the reactor is 1:0.9 to 1:10.5; In the case where the mixed gas contains water vapor, the volume ratio of the aldehyde containing at least one carbon-carbon double bond and the water vapor input into the reactor is 1:1 to 1:

5.

10. The method of claim 1, wherein the reaction does not produce hydrocyanic acid.