3D printing material and application thereof

By introducing low-melting dihydroxyalkyl terephthalate and its oligomers and appropriate amounts of impurities into the recycling PET resin, the problem of high-temperature aging and impurities in 3D printing is solved, and the processing performance of the material is improved and mechanical properties have expanded their application areas.

CN119060511APending Publication Date: 2024-12-03FUJIAN HUAFENG NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410994906.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, when recycling PET materials for 3D printing, there are problems such as high-temperature aging and degradation and difficult application of by-product PET powder impurities, resulting in reduced mechanical properties and limited application.

Method used

Use low-melting dihydroxyalkyl terephthalate and its oligomers to blend with recovered PET resin to adjust melt viscosity and fluidity, reduce the impact of mechanical properties, and introduce appropriate amounts of impurities to improve crystallization behavior, forming suitable for 3D Combination of printing materials.

Benefits of technology

It improves the processing properties and mechanical properties of the recycling of PET resin, extends the application field of materials, avoids the aging and degradation problems caused by high-temperature processing, and broadens its application in 3D printing materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a 3D (three-dimensional) printing material and application thereof, the 3D printing material comprises the following raw material components in percentage by weight: 1-45% of dihydroxyalkyl terephthalate and oligomer thereof, and the balance of PET (polyethylene terephthalate) resin; the melting point of the dihydroxyalkyl terephthalate and the oligomer thereof does not exceed 210 DEG C; the weight ratio of the recycled PET resin in the PET resin is not less than 20%. The low-melting-point dihydroxyalkyl terephthalate and the oligomer thereof are introduced into the PET matrix resin containing the recycled PET resin for blending, so that in the additive manufacturing process, on one hand, the melt viscosity can be reduced at the melting temperature to adjust the melt fluidity, and the processability of the recycled PET resin for the 3D printing material is improved; on the other hand, the dihydroxyalkyl terephthalate and the oligomer thereof have good compatibility with a PET resin matrix, and the influence on the mechanical property of a subsequent 3D printing product can be reduced. By improving the performance of the recycled PET resin, recycling of the recycled PET resin is efficiently achieved, and environmental protection and sustainable development are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a 3D printing material and application thereof. Background Art

[0002] PET is a thermoplastic with advantages such as light weight, high chemical stability and good mechanical properties. Therefore, it is widely used in food packaging, fiber and electrical insulation materials. The global annual PET production exceeds 700 million tons. 7 t, of which about 21,000 kt is used for food packaging bottles and about 46,000 kt is used for chemical fibers. However, the recycling rate of these PET products after they are discarded is only 14%. A large amount of waste plastics will inevitably cause serious pollution to the ecological environment. Therefore, finding a way to recycle waste PET with higher added value has important social value and practical significance.

[0003] In the prior art, it is proposed to recycle waste PET for the production of 3D printing materials to solve the problem of its recycling. For example, Chinese patent CN116394485A discloses a method for recycling polyester textiles to produce fused deposition 3D printing wires. It uses a hot pressing molding process to recycle polyester textiles, which not only overcomes the problem that waste textiles are loose and difficult to process, but also improves the extrusion processing stability of recycled PET materials; using epoxy tackifiers, the elasticity of the recycled PET melt is improved, and the extrusion processing stability of the recycled PET material and the mechanical properties of 3D printed parts are improved. However, the fused deposition molding method has the following problems:

[0004] (1) When using wire as the printing material for fused deposition modeling, the wire will inevitably age and degrade during the high-temperature processing of the wire, resulting in a decrease in the mechanical properties of the final product.

[0005] (2) Recycled chemical fiber PET is used as 3D printing filament, which has high requirements on the quality of recycled PET and its application is limited.

[0006] At present, when PET bottle flakes are recycled by physical methods, the by-product PET powder produced in each process section (mainly the hot washing process section and the cold washing process section) will inevitably carry trace impurities, making it difficult to apply to high-demand wire manufacturing. At the same time, if it is directly used to produce 3D printing materials, there will be problems such as not meeting the plasticizing and extrusion conditions of 3D printing materials, which is not conducive to additive manufacturing. Therefore, it is very necessary to propose a method that can effectively solve the problem of recycling by-product PET powder and further expand its application field. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a 3D printing material and application thereof.

[0008] The technical solution adopted by the present invention is:

[0009] In a first aspect, the present invention provides a 3D printing material, wherein the raw material components, by 100% by weight, include: 1-45% dihydroxyalkyl terephthalate and its oligomers, and the balance is PET resin;

[0010] The melting point of the dihydroxyalkyl terephthalate and its oligomers is not more than 210°C;

[0011] The weight proportion of the recycled PET resin in the PET resin is not less than 20%.

[0012] The 3D printing material proposed by the present invention is a PET matrix resin containing recycled PET resin. By introducing low-melting-point dihydroxyalkyl terephthalate and its oligomers into the PET matrix resin, the low-melting-point dihydroxyalkyl terephthalate and its oligomers are blended. In the process of additive manufacturing, on the one hand, the melt viscosity can be reduced at the melting temperature to adjust the melt fluidity, thereby improving the processing performance of the recycled PET resin for 3D printing materials; on the other hand, the dihydroxyalkyl terephthalate and its oligomers have good compatibility with the PET resin matrix, which can reduce the impact on the mechanical properties of subsequent 3D printed products. The present invention improves the performance of the recycled PET resin and efficiently realizes its recycling and reuse, which is conducive to environmental protection and sustainable development.

[0013] Preferably, the raw material components further include 7-9% of an auxiliary agent, and the auxiliary agent is selected from one or a combination of two or more of an antioxidant, a nucleating agent, an ultraviolet light absorber, a lubricant, a matting powder and a pigment.

[0014] Preferably, the impurity content in the recycled PET resin is not less than 0.1wt% and not more than 1wt%.

[0015] Preferably, the impurities are nano-sized and are selected from one or a combination of two or more of inorganic fillers, metals, metal oxides and organic carboxylates.

[0016] Preferably, the weight percentage of the dihydroxyalkyl terephthalate and its oligomers is not less than 10%.

[0017] Preferably, the general formula of the dihydroxyalkyl terephthalate is HOROCOPhCOOROH, wherein Ph represents phenylene and R is selected from C1-C4 alkyl.

[0018] Preferably, the dihydroxyalkyl terephthalate and oligomers thereof are selected from one or a combination of two or more of dihydroxyethyl terephthalate and oligomers thereof, dihydroxypropyl terephthalate and dihydroxybutyl terephthalate.

[0019] In a second aspect, the present invention provides an application of a 3D printing material as described in any of the above technical solutions in the field of molten particle manufacturing.

[0020] Preferably, the process parameters for manufacturing the molten particles are: nozzle diameter of 0.5-2 mm, melting temperature of 245-270° C., nozzle temperature of 250-260° C., hot bed temperature of 60° C., and printing speed of 30-60 mm / s.

[0021] The 3D printing material of the present invention is added with low-melting-point dihydroxyalkyl terephthalate and its oligomers, which reduces the melting range and / or viscosity of the 3D printing material. The 3D printing material can be directly manufactured into melt particles, avoiding the aging and degradation caused by high-temperature processing pretreatment of wire forming, thereby causing the mechanical properties of the 3D printed product to decrease. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further illustrated and described below through specific implementation methods.

[0023] In one aspect, the present invention provides a 3D printing material, wherein the raw material components, by weight, include: 1-45% dihydroxyalkyl terephthalate and its oligomers, and the balance is PET resin;

[0024] The melting point of dihydroxyalkyl terephthalate and its oligomers shall not exceed 210°C;

[0025] The weight proportion of recycled PET resin in the PET resin is not less than 20%.

[0026] In the present invention, the weight percentage of dihydroxyalkyl terephthalate and its oligomer is 1-45%, for example, it can be any value among 1%, 5%, 8%, 10%, 15%, 18%, 20%, 22%, 25%, 27%, 30%, 32%, 35%, 40%, 45%, etc., but not limited to the above. However, the amount of dihydroxyalkyl terephthalate and its oligomer should not be too high, otherwise it may cause insufficient melt viscosity or insufficient strength of the printed material, thereby having an adverse effect on melt additive manufacturing. In the present invention, the melting point of dihydroxyalkyl terephthalate and its oligomers is not more than 210°C, for example, it can be any value of 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, etc., but not limited to the above. The melting point of dihydroxyalkyl terephthalate and its oligomers should not be too high, otherwise it is not conducive to reducing the melting point and viscosity of 3D printing materials, and 3D printing materials are still prone to thermal degradation at high temperatures, and product performance is reduced; at the same time, the melting point of dihydroxyalkyl terephthalate and its oligomers should not be too low, otherwise it will cause a serious decrease in mechanical properties and is not conducive to extrusion processing.

[0027] In a preferred embodiment of the present invention, the raw material components also include 7-9% of an auxiliary agent, and the auxiliary agent is selected from one or a combination of two or more of an antioxidant, a nucleating agent, an ultraviolet light absorber, a lubricant, a matting powder and a pigment. In the present invention, auxiliary agents can be appropriately introduced to cooperate with each other to better improve the product's antioxidant properties, mechanical properties, processing properties and other aspects. Conventional auxiliary agents in the field can be used, and can be directly purchased and used from the market without special restrictions. For example, the antioxidant can be a hindered phenol antioxidant 1010, a phosphite antioxidant 168 or a mixture of the two; the nucleating agent can be an inorganic nucleating agent or an organic nucleating agent, preferably an inorganic nucleating agent, and more preferably a hydroxide, such as aluminum hydroxide or magnesium hydroxide; the lubricant can be at least one of PP wax, stearic acid, stearate, etc.

[0028] In a preferred embodiment of the present invention, the impurity content in the recycled PET resin is not less than 0.1wt% and not more than 1wt%. In the present invention, the inventors found that the presence of an appropriate amount of impurities in the recycled PET resin does not affect the quality and performance of the products used in 3D printing, but can improve the mechanical properties. For example, the impurity content in the recycled PET resin can be any value of 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, etc., without special restrictions. However, the impurity content must be appropriate, too much or too little will affect the effect.

[0029] In a preferred embodiment of the present invention, the impurities are nanometer-sized and are selected from one or a combination of two or more of inorganic fillers, metals, metal oxides and organic carboxylates. In the present invention, the impurities in the recycled PET resin can act as heterogeneous nucleating agents, improve the crystallization behavior of the recycled PET resin, and thus improve the mechanical properties of the product, such as shrinkage resistance, bending strength, etc. For example, the inorganic filler can be silicon dioxide, titanium dioxide, calcium carbonate, etc.; the metal can be magnetic metal particles, such as iron, etc.; the metal oxide can be zinc oxide, magnesium oxide, iron oxide, etc.; the organic carboxylate can be benzoate, such as potassium benzoate, sodium benzoate, etc., all of which are nanometer-sized.

[0030] In a preferred embodiment of the present invention, the weight percentage of dihydroxyalkyl terephthalate and its oligomers is not less than 10%. In the present invention, further screening the dosage range of dihydroxyalkyl terephthalate and its oligomers is conducive to better reducing the melt viscosity of 3D printing materials and improving fluidity. If the dosage of dihydroxyalkyl terephthalate and its oligomers is too low, the expected effect cannot be achieved. For example, the weight percentage of dihydroxyalkyl terephthalate and its oligomers can be any value of 10%, 12%, 15%, 18%, 20%, 22%, 25%, 27%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, etc., but is not limited to the above-mentioned ones.

[0031] In a preferred embodiment of the present invention, the general formula of dihydroxyalkyl terephthalate is HOROCOPhCOOROH, wherein Ph represents phenylene and R is selected from C1-C4 alkyl.

[0032] In a more preferred embodiment of the present invention, the dihydroxyalkyl terephthalate and its oligomers are selected from one or a combination of two or more of dihydroxyethyl terephthalate and its oligomers, dihydroxypropyl terephthalate and dihydroxybutyl terephthalate. In the present invention, for example, the dihydroxyethyl terephthalate oligomer can be a dimer, trimer, tetramer, etc. of dihydroxyethyl terephthalate. When the dihydroxyalkyl terephthalate is selected from dihydroxyethyl terephthalate, dimer of dihydroxyethyl terephthalate, trimer of dihydroxyethyl terephthalate, dihydroxypropyl terephthalate, and dihydroxybutyl terephthalate, the melting points thereof are approximately 110°C, 170°C, 200°C, 81°C, and 94°C, respectively, which are much lower than the melting point of 250-255°C of conventional PET resin, and can well reduce the melt viscosity, regulate the melt fluidity of 3D printing materials at high temperatures, and be beneficial to plasticizing extrusion; and it has a similar chemical structure to the matrix PET resin, has good compatibility, and can make the 3D printed products have higher mechanical properties.

[0033] Another aspect of the present invention provides an application of a 3D printing material according to any of the above technical solutions in the field of molten particle manufacturing.

[0034] In a preferred embodiment of the present invention, the process parameters for manufacturing molten particles are: nozzle diameter of 0.5-2mm, melting temperature of 245-270°C, nozzle temperature of 250-260°C, hot bed temperature of 60°C, and printing speed of 30-60mm / s. For example, the nozzle diameter can be any value of 0.5mm, 1.0mm, 1.5mm, 2mm, etc., the nozzle temperature can be any value of 250°C, 252°C, 254°C, 256°C, 258°C, 260°C, etc., the melting temperature can be any value of 245°C, 250°C, 255°C, 260°C, 265°C, 270°C, etc., and the printing speed can be any value of 30mm / s, 40mm / s, 45mm / s, 50mm / s, etc. Among them, the melting temperature can be specifically selected according to different heating zones. Traditional 3D printing wires require high-temperature processing of raw materials in advance, but this inevitably leads to degradation of raw materials, resulting in a decrease in material performance. However, with the 3D printing material of the present invention, melt extrusion can be directly performed, avoiding the adverse effects of degradation and being closer to the chemical and physical properties of plastics used in injection molding.

[0035] Example 1

[0036] A 3D printing material, wherein the raw material components are 100% by weight, including: 30% of dihydroxyethyl terephthalate, 55% of recycled PET resin (containing 0.1wt% of impurities, which are a mixture of nano-scale calcium carbonate, Fe and zinc oxide), and the remainder is PET resin.

[0037] When it is used for molten particle manufacturing, the process parameters are: nozzle diameter is 1.5mm, nozzle temperature is 257℃, melting temperatures of zones one to three are 250℃, 255℃, and 258℃ respectively, hot bed temperature is 60℃, and printing speed is 50mm / s.

[0038] Example 2

[0039] The difference between this embodiment and embodiment 1 is that the impurity content is different, and the recycled PET resin containing 0.1 wt% impurities in embodiment 1 is replaced by an equal amount of recycled PET resin containing 1 wt% impurities. The remaining steps remain unchanged.

[0040] Example 3

[0041] The difference between this embodiment and embodiment 2 is that the dihydroxyethyl terephthalate in embodiment 2 is replaced by dihydroxypropyl terephthalate in an equal weight percentage. The remaining steps remain unchanged.

[0042] Example 4

[0043] The difference between this embodiment and embodiment 2 is that the dihydroxyethyl terephthalate in embodiment 2 is replaced by dihydroxybutyl terephthalate in an equal weight percentage. The remaining steps remain unchanged.

[0044] Example 5

[0045] The difference between this embodiment and embodiment 2 is that the dihydroxyethyl terephthalate in embodiment 2 is replaced by the dimer of dihydroxyethyl terephthalate in an equal weight percentage. The other steps remain unchanged.

[0046] Example 6

[0047] The difference between this embodiment and embodiment 2 is that the dihydroxyethyl terephthalate in embodiment 2 is replaced by a trimer of dihydroxyethyl terephthalate in an equal weight percentage. The remaining steps remain unchanged.

[0048] Example 7

[0049] The difference between this embodiment and embodiment 2 is that 30% of dihydroxyethyl terephthalate in embodiment 2 is replaced by 10% of dihydroxyethyl terephthalate, and the remaining 20% ​​is supplemented by PET resin. The other steps remain unchanged.

[0050] Example 8

[0051] The difference between this embodiment and embodiment 2 is that in embodiment 2, 30% of dihydroxyethyl terephthalate is replaced by 45% of dihydroxyethyl terephthalate, and 15% of PET resin is reduced. The other steps remain unchanged.

[0052] Example 9

[0053] The difference between this embodiment and embodiment 2 is that 8% of auxiliary agents (0.2% antioxidant 1010, 2.85% aluminum hydroxide, 0.15% ultraviolet light absorber, 0.4% TS-100, 4.4% PP wax) are added, and the PET resin is reduced by the same weight percentage. The other steps remain unchanged.

[0054] Comparative Example 1

[0055] The difference between this comparative example and Example 2 is that the impurity content is different, and the recycled PET resin containing 1 wt% impurities in Example 2 is replaced by an equal amount of recycled PET resin containing 1.5 wt% impurities. The remaining steps remain unchanged.

[0056] Comparative Example 2

[0057] The difference between this comparative example and Example 2 is that the impurity content is different, and the recycled PET resin containing 1 wt% impurities in Example 2 is replaced by an equal amount of recycled PET resin containing 0.05 wt% impurities. The remaining steps remain unchanged.

[0058] Comparative Example 3

[0059] The difference between this comparative example and Example 2 is that dihydroxyethyl terephthalate is not added, and PET resin is used to make up the difference in weight percentage. The other steps remain unchanged.

[0060] Comparative Example 4

[0061] The difference between this comparative example and Example 2 is that the dihydroxyethyl terephthalate in Example 2 is replaced by diethyl terephthalate in an equal weight percentage. The remaining steps remain unchanged.

[0062] Comparative Example 5

[0063] The difference between this comparative example and Example 4 is that the dibutyl terephthalate in Example 4 is replaced by dibutyl terephthalate in an equal weight percentage. The remaining steps remain unchanged.

[0064] The performance test results of Examples 1-9 and Comparative Examples 1-5 are shown in Table 1 below.

[0065] Viscosity test method: The melt viscosity was measured using a capillary rheometer, the capillary aspect ratio was 40:1, the test temperature was 270°C, and the shear rate was 1000s -1 .

[0066] Table 1

[0067] Viscosity (dl / g) Bending strength(MPa) Tensile strength(MPa) Example 1 0.69 82.4 60.0 Example 2 0.68 86.3 64.5 Example 3 0.66 83.6 61.6 Example 4 0.65 82.1 60.9 Example 5 0.72 86.8 64.8 Example 6 0.73 87.2 65.2 Example 7 0.73 88.5 66.9 Example 8 0.66 81.1 59.7 Example 9 0.65 87.8 65.3 Comparative Example 1 0.71 79.9 58.3 Comparative Example 2 0.70 78.7 57.8 Comparative Example 3 0.81 89.9 68.7 Comparative Example 4 0.56 65.2 46.6 Comparative Example 5 0.54 53.7 41.2

[0068] It can be seen from the data in Table 1 that the 3D printing material of the present invention enhances the melt fluidity based on the recycled PET resin by introducing low-melting-point dihydroxyalkyl terephthalate, stabilizes the extrusion speed, and because a small amount of impurities are entrained in the recycled PET resin, it can also improve the crystallization behavior and mechanical properties of the material, thereby broadening the application field of the recycled PET resin.

[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A 3D printing material, the raw material components are 100% by weight, including: 1-45% dihydroxyalkyl terephthalate and its oligomers, the balance is PET resin; The melting point of the dihydroxyalkyl terephthalate and its oligomers is not more than 210°C; The weight proportion of the recycled PET resin in the PET resin is not less than 20%.

2. The 3D printing material according to claim 1, characterized in that: The raw material components also include 7-9% of auxiliary agents, and the auxiliary agents are selected from one or a combination of two or more of antioxidants, nucleating agents, ultraviolet light absorbers, lubricants, matting powders and pigments.

3. The 3D printing material according to claim 1, characterized in that: The impurity content in the recycled PET resin is not less than 0.1wt% and not more than 1wt%.

4. The 3D printing material according to claim 1, characterized in that: The impurities are nanometer-sized and are selected from one or a combination of two or more of inorganic fillers, metals, metal oxides and organic carboxylates.

5. The 3D printing material according to claim 1, characterized in that: The weight percentage of the dihydroxyalkyl terephthalate and its oligomer is not less than 10%.

6. The 3D printing material according to claim 1, characterized in that: The general formula of the dihydroxyalkyl terephthalate is HOROCOPhCOOROH, wherein Ph represents phenylene and R is selected from C1-C4 alkyl.

7. The 3D printing material according to claim 6, characterized in that: The dihydroxyalkyl terephthalate and its oligomers are selected from one or a combination of two or more of dihydroxyethyl terephthalate and its oligomers, dihydroxypropyl terephthalate and dihydroxybutyl terephthalate.

8. An application of the 3D printing material according to any one of claims 1 to 7 in the field of molten particle manufacturing.

9. The use of the 3D printing material according to claim 8, characterized in that: The process parameters for manufacturing the molten particles are: nozzle diameter of 0.5-2 mm, melting temperature of 245-270° C., nozzle temperature of 250-260° C., hot bed temperature of 60° C., and printing speed of 30-60 mm / s.