Insulating heat-conducting nano-particles as well as preparation method and application thereof

By modifying the aminobenzoic acid and aminosilane coupling agent on the aluminum trioxide particles, high-insulating and high-thermal conductivity nanoparticles are formed, which solves the problem of insufficient electric breakdown performance of aluminum trioxide in electronic equipment, and realizes the It has higher insulation and thermal conductivity, suitable for the needs of modern electronic equipment.

CN119060541APending Publication Date: 2024-12-03BEIJING DISCOVERY INTELLIGENT MFG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411194293.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing aluminum trioxide limits the ability of electrons in highly thermally conductive insulating devices, resulting in insufficient performance of materials in electrical breakdown and unable to effectively meet the demands of modern electronic devices for high-insulating and high-thermal conductive materials.

Method used

By ultrasonic stirring of aminobenzoic acid and aminosilane coupling agent with aluminum trioxide particles in toluene and ethanol solutions, functionalized nanoparticles are formed, and their insulation and thermal conductivity are enhanced, and high insulation and high thermal conductivity are prepared. .

Benefits of technology

It significantly improves the insulation and thermal conductivity of thermal grease, expands its application range, and enhances its resistance to external stress and chemical stress, making it suitable for large-scale production and industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060541A_ABST
    Figure CN119060541A_ABST
Patent Text Reader

Abstract

The invention relates to insulating heat-conducting nanoparticles as well as a preparation method and application thereof. The preparation method comprises the following steps: adding aminobenzoic acid (m-ABA) into a toluene solution, and stirring for dissolving; adding an amino silane coupling agent (KH-550) solution, and uniformly stirring; stirring the solution at 50-70 DEG C, then adding aluminum oxide particles, and performing ultrasonic stirring to form colloid; adding ethanol, and performing ultrasonic stirring to obtain a functionalized nanoparticle material; and filtering, washing and drying the nano-particle material to obtain the final nano-particle material. According to the improved nano-particle material, the good heat conduction characteristic is reserved, the insulating capacity of the heat-conducting silicone grease can be improved, the application space of the heat-conducting silicone grease is expanded, and the application range of the heat-conducting silicone grease is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of material technology, and specifically relates to a high-insulation and high-thermal-conductivity nanoparticle and a preparation method thereof, which can be applied to electronic equipment, energy transportation and other fields. Background Art

[0002] With the in-depth development of 5G technology and electronic information technology in my country, the integration of electronic equipment is getting higher and higher. In order to ensure the safe operation of the equipment, it is necessary to improve the insulation performance of high thermal conductivity materials. Aluminum oxide plays a key role in the heat transfer and sealing performance of equipment due to its excellent thermal conductivity and easy processing performance. However, in the equipment, the insufficient ability of aluminum oxide to restrict electrons leads to electrical breakdown of the material, which limits the application of aluminum oxide in high thermal conductivity insulation devices.

[0003] The most basic and important function of high thermal conductivity insulating materials is to insulate charged conductors from each other. At the same time, under certain conditions, it is necessary to exert certain mechanical properties to resist external stress damage and be able to withstand certain thermal stress and chemical stress. The following requirements are required for this: high electrical insulation performance, low dielectric loss, and appropriate dielectric constant. It can achieve small size and low cost under less material conditions. At the same time, insulating materials are generally in a high heat environment and have certain thermal stability and heat transfer capabilities. Therefore, the development of a nanoparticle with high insulation and high thermal conductivity is of advanced significance for the development of modern equipment and technology. Summary of the invention

[0004] Technical problem to be solved: The present invention provides an insulating thermally conductive nanoparticle and a preparation method and application thereof. Compared with the aluminum oxide particles used on the market, the nanoparticle has higher insulation performance and a lower dielectric constant, while maintaining the dielectric constant unchanged. It has a replicable and industrializable basis and is conducive to the potential for large-scale production and preparation.

[0005] Technical solution: A method for preparing insulating thermally conductive nanoparticles, according to the following proportions, the preparation steps are: a. adding 0.08 mol to 0.3 mol of aminobenzoic acid (m-ABA) to 50 mL of toluene solution and stirring to dissolve; b. adding 0.1 mol to 0.8 mol of aminosilane coupling agent (KH-550) solution in step a and stirring evenly; c. placing the solution in step b at 50-70° C. and stirring, then adding 0.1 g to 1 g of aluminum oxide particles and ultrasonically stirring to form a colloid; d. in step c, adding 10 mL of ethanol and ultrasonically stirring to obtain a functionalized nanoparticle material; e. filtering the nanoparticle material in step d, washing, and drying to obtain the final nanoparticle material.

[0006] Preferably, the amount of the aminobenzoic acid is 0.15 mol.

[0007] Preferably, the amount of KH-550 is 0.5 mol.

[0008] Preferably, the amount of aluminum oxide used is 0.1 g.

[0009] The preferred embodiment is to put 0.15 mol of aminobenzoic acid (m-ABA) into 50 mL of toluene solution and stir to dissolve, then add 0.6 mol of aminosilane coupling agent (KH-550) solution and stir evenly, then place the above solution at 60°C and stir for 3 hours, then add 0.1 g of aluminum oxide particles and ultrasonically stir to form a colloid, then add 10 mL of ethanol and ultrasonically stir for 24 hours to obtain a functionalized nanoparticle material; finally, the nanoparticle material in the above solution is filtered, washed, and dried to obtain the final nanoparticle material.

[0010] The insulating thermally conductive nanoparticles obtained by the above preparation method.

[0011] Application of the above insulating thermally conductive nanoparticles in the preparation of insulating devices.

[0012] During the research process, the applicant found that toluene alone could not well infiltrate the aluminum oxide particle material. After adding ethanol, the aluminum oxide infiltration was deeper, which prompted more aluminum oxide surfaces to be modified, and the insulation and thermal conductivity of the thermal grease could be improved as a whole.

[0013] Beneficial effects: Aluminum oxide has good thermal conductivity, but increasing the insulation properties of particles through nano-modification will reduce the thermal conductivity of the material, thereby increasing the thermal resistance of thermal grease and reducing the heat transfer rate. Our improved nano-particle material not only retains good thermal conductivity, but also improves the insulation capacity of thermal grease, expands the application space of thermal grease, and increases the scope of use of thermal grease. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 : Actual picture of aluminum oxide prepared in Example 2.

[0015] Figure 2 : The breakdown voltage data diagram of the modified aluminum oxide mixed silicone oil in each embodiment.

[0016] Figure 3 : The breakdown voltage data of modified aluminum oxide and silicone oil in each embodiment.

[0017] Figure 4 : The microstructure of aluminum oxide in Example 2.

[0018] Test method: The thermal conductivity test method is Hotdisk equipment test, and the test basis is ISO 22007-2; the breakdown voltage test standard is ASTM-D149. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with specific embodiments.It should be noted that each of the following embodiments is exemplary, and is not intended to limit the scope of the present invention.After reading content of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the claims of the present application equally.

[0020] Example 1

[0021] 0.08 mol of aminobenzoic acid (m-ABA) was placed in 50 mL of toluene solution and stirred to dissolve, and then 0.6 mol of aminosilane coupling agent (KH-550) solution was added and stirred evenly. Next, the above solution was placed at 60°C and stirred for 3 hours, and then 0.5 g of aluminum oxide particles was added and ultrasonically stirred to form a colloid, and then 10 mL of ethanol was added and ultrasonically stirred for 24 hours to obtain a functionalized nanoparticle material; finally, the nanoparticle material in the above solution was filtered, washed, and dried to obtain the final nanoparticle material.

[0022] Example 2

[0023] 0.15 mol of aminobenzoic acid (m-ABA) was placed in 50 mL of toluene solution and stirred to dissolve, and then 0.6 mol of aminosilane coupling agent (KH-550) solution was added and stirred evenly. Next, the above solution was placed at 60°C and stirred for 3 hours, and then 0.5 g of aluminum oxide particles was added and ultrasonically stirred to form a colloid, and then 10 mL of ethanol was added and ultrasonically stirred for 24 hours to obtain functionalized nanoparticle material; finally, the nanoparticle material in the above solution was filtered, washed, and dried to obtain the final nanoparticle material.

[0024] Example 3

[0025] 0.3 mol of aminobenzoic acid (m-ABA) was placed in 50 mL of toluene solution and stirred to dissolve, and then 0.6 mol of aminosilane coupling agent (KH-550) solution was added and stirred evenly. Next, the above solution was placed at 60°C and stirred for 3 hours, and then 0.5 g of aluminum oxide particles was added and ultrasonically stirred to form a colloid, and then 10 mL of ethanol was added and ultrasonically stirred for 24 hours to obtain a functionalized nanoparticle material; finally, the nanoparticle material in the above solution was filtered, washed, and dried to obtain the final nanoparticle material.

[0026] In Examples 1 to 3, we prepared a high insulation and high thermal conductivity nanoparticle material using the mass of aminotoluic acid (m-ABA) as a variable to obtain the amount of material for preparing the optimal m-ABA powder for high insulation nanoparticles.

[0027] The experimental results are summarized as follows:

[0028]

[0029] Example 4

[0030] 0.15 mol of aminobenzoic acid (m-ABA) was placed in 50 mL of toluene solution and stirred to dissolve, and then 0.1 mol of aminosilane coupling agent (KH-550) solution was added and stirred evenly. Next, the above solution was placed at 60°C and stirred for 3 hours, and then 0.5 g of aluminum oxide particles was added and ultrasonically stirred to form a colloid. Subsequently, 10 mL of ethanol was added and ultrasonically stirred for 24 hours to obtain a functionalized nanoparticle material. Finally, the nanoparticle material in the above solution was filtered, washed, and dried to obtain the final nanoparticle material.

[0031] Example 5

[0032] 0.15 mol of aminobenzoic acid (m-ABA) was placed in 50 mL of toluene solution and stirred to dissolve, and then 0.8 mol of aminosilane coupling agent (KH-550) solution was added and stirred evenly. Next, the above solution was placed at 60°C and stirred for 3 hours, and then 0.5 g of aluminum oxide particles was added and ultrasonically stirred to form a colloid, and then 10 mL of ethanol was added and ultrasonically stirred for 24 hours to obtain functionalized nanoparticle material; finally, the nanoparticle material in the above solution was filtered, washed, and dried to obtain the final nanoparticle material.

[0033] In Examples 2, 4, and 5, we prepared a highly insulating granular material by using the amount of aminosilane coupling agent as a variable to obtain the optimal amount of KH-550 for preparing the granular material.

[0034] The experimental results are summarized as follows:

[0035]

[0036] Example 6

[0037] 0.15 mol of aminobenzoic acid (m-ABA) was placed in 50 mL of toluene solution and stirred to dissolve, and then 0.6 mol of aminosilane coupling agent (KH-550) solution was added and stirred evenly. Next, the above solution was placed at 60°C and stirred for 3 hours, and then 0.1 g of aluminum oxide particles was added and ultrasonically stirred to form a colloid. Subsequently, 10 mL of ethanol was added and ultrasonically stirred for 24 hours to obtain a functionalized nanoparticle material. Finally, the nanoparticle material in the above solution was filtered, washed, and dried to obtain the final nanoparticle material.

[0038] Example 7

[0039] 0.15 mol of aminobenzoic acid (m-ABA) was placed in 50 mL of toluene solution and stirred to dissolve, and then 0.6 mol of aminosilane coupling agent (KH-550) solution was added and stirred evenly. Next, the above solution was placed at 60°C and stirred for 3 hours, and then 1 g of aluminum oxide particles was added and ultrasonically stirred to form a colloid. Subsequently, 10 mL of ethanol was added and ultrasonically stirred for 24 hours to obtain a functionalized nanoparticle material. Finally, the nanoparticle material in the above solution was filtered, washed, and dried to obtain the final nanoparticle material.

[0040] In Examples 2, 6, and 7, we used the mass of aluminum oxide powder as a variable to prepare a high-insulation nanoparticle material to obtain the mass of the optimal aluminum oxide powder for preparing nanomaterials. A high-insulation nanoparticle material was prepared according to the above preparation method using aluminum oxide powder with masses of 0.1 g, 0.5 g, and 1 g.

[0041] The experimental results are summarized as follows:

[0042]

Claims

1. A method for preparing insulating thermally conductive nanoparticles, characterized in that: According to the following proportions, the preparation steps are as follows: a. Add 0.08 mol~0.3 mol of aminobenzoic acid (m-ABA) into 50 mL of toluene solution and stir to dissolve; b. Add 0.1 mol~0.8 mol of aminosilane coupling agent (KH-550) solution in step a and stir evenly; c. Place the solution in step b at 50-70°C and stir, then add 0.1g~1g of aluminum oxide particles and stir ultrasonically to form a colloid; d. In step c, add 10 mL of ethanol and stir ultrasonically to obtain a functionalized nanoparticle material; e. Filter the nanoparticle material in step d, wash, and dry to obtain the final nanoparticle material.

2. The method for preparing insulating thermally conductive nanoparticles according to claim 1, characterized in that: The amount of aminobenzoic acid used is 0.15 mol.

3. The method for preparing insulating thermally conductive nanoparticles according to claim 1, characterized in that: The usage of KH-550 is 0.5 mol.

4. The method for preparing insulating thermally conductive nanoparticles according to claim 1, characterized in that: The amount of aluminum oxide used is 0.1 g.

5. The method for preparing insulating thermally conductive nanoparticles according to claim 1, characterized in that: Put 0.15 mol of aminobenzoic acid (m-ABA) into 50 mL of toluene solution and stir to dissolve, then add 0.6 mol of aminosilane coupling agent (KH-550) solution and stir evenly. Then place the above solution at 60°C and stir for 3 hours, then add 0.1 g of aluminum oxide particles and stir ultrasonically to form a colloid, then add 10 mL of ethanol and stir ultrasonically for 24 hours to obtain functionalized nanoparticle material; finally, filter the nanoparticle material in the above solution, wash, and dry to obtain the final nanoparticle material.

6. The insulating thermally conductive nanoparticles obtained by the preparation method according to any one of claims 1 to 5.