Method for preparing coating with low emissivity and low near-infrared reflectivity by cell crushing method
The preparation process of low-infrared emissivity coating is simplified by cell pulverization enhancement method, solving the problems of complexity of traditional methods and high energy consumption, and achieving low infrared, low gloss, low near-infrared reflectivity coatings with better infrared Compatible with multi-spectrum stealth effects.
Patent Information
- Application Number
- CN202411351833.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing low-infrared emissivity coating preparation process is complex, with many process steps, high energy consumption, and high gloss and high near-infrared reflectivity of 1.06μm, making it difficult to compatible.
Using cell pulverization enhancement method, the cell pulverization enhancement treatment was performed by high-energy planetary ball milling machine ball milling graphite and sheet Al powder, combined with butyl acetate and KH560/DOP as diluents and modifiers, and ultra-high frequency oscillation sound waves were used to perform cell pulverization enhancement dispersion treatment, simplifying the Process steps and adjust the viscosity of the coating to achieve low emissivity, low gloss, and low near infrared reflectivity coating preparation.
It significantly reduces infrared emissivity, glossiness and 1.06μm near-infrared reflectivity, simplifies process steps, reduces energy consumption and production costs, and improves the infrared and multi-spectrum compatible stealth effect of the coating.
Smart Images

Figure CN119060610A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fine chemical industry, in particular to a method for preparing a coating with low emissivity and low near-infrared reflectivity by a cell crushing method. Background Art
[0002] In recent years, in order to meet the needs of high maneuverability and high-speed penetration, the flight speeds of various aircraft such as fighters and missiles have become faster and faster. During the high-speed flight of various aircraft, due to the heat emitted by the engine and the heat generated by the friction between the fuselage and the air, the infrared radiation characteristics of the aircraft are very obvious under the cold background conditions of the sky, which can easily cause various aircraft to be locked and destroyed by enemy infrared detection equipment. Therefore, low infrared emissivity materials that can significantly reduce the infrared radiation intensity of various aircraft have received great attention from domestic and foreign experts. According to the preparation method, material structure and material type, low infrared emissivity materials include nanocomposite films, single (multilayer) film structure materials, core-shell structure composite materials, photonic crystals, composite coatings and other types. Among them, resin-based composite coatings composed of various resin substrates and flaky metal pigments are the research hotspots in the field of low infrared emissivity materials. This type of coating material is also considered to be the most promising low infrared emissivity material in large-scale engineering applications.
[0003] The two core technical indicators of resin-based low infrared emissivity coatings are low infrared emissivity and low gloss. At the same time, in order to cope with the threat of laser detection and guidance technology that is currently widely used, it is also necessary to have a low reflectivity characteristic of 1.06μm near-infrared. The above technical indicators are mainly related to the composition of the coating, the composition structure of the functional filler, the surface state, the arrangement state and the dispersion state. Existing research mainly focuses on the design of coating formula composition and performance research. By adjusting the formulation composition of the coating, the infrared emissivity and gloss of the coating can be controlled and optimized. However, there are few reports on the multifunctional (low emissivity, low gloss, low near-infrared reflectivity) composite modification of flaky metal powders and the use of external strengthening treatment to improve the surface state of the coating and the dispersion state and arrangement state of the functional filler in the coating.
[0004] In addition, the existing low infrared emissivity coating preparation process involves complex processes such as coating stirring, high-speed dispersion, grinding (sand grinding), etc., with many process steps and high energy consumption. Therefore, it is also necessary to design corresponding technical solutions to solve this problem. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the shortcomings of the prior art, the present invention provides a method for preparing a low-emissivity, low-gloss, and low-near-infrared reflectivity compatible coating by a cell crushing enhancement method, which solves the compatibility problem of the traditional method for preparing low-emissivity coatings with high gloss and high 1.06μm near-infrared reflectivity. At the same time, it solves the technical problem that the preparation process of low-infrared emissivity coatings involves complex processes such as coating stirring, high-speed dispersion, grinding (sand grinding), many process steps, and high energy consumption.
[0007] (II) Technical solution
[0008] To achieve the above objectives, the present invention is implemented by the following technical scheme: a method for preparing a low-emissivity, low-gloss, low-near-infrared reflectivity compatible coating by a cell crushing enhancement method, the method steps comprising the following:
[0009] S1. Use a test-grade standard tinplate as the substrate, polish the substrate with 200-400 grit sandpaper to make it have a certain roughness, and wipe the substrate clean with disposable tissue dipped in alcohol for later use;
[0010] S2. Milling graphite and flaky Al powder for 30 to 60 minutes at a speed of 400 to 800 r / min using a high-energy planetary ball mill to obtain graphite-modified Al powder, and weighing appropriate amounts of resin matrix and graphite-modified Al powder in a clean disposable plastic cup in a mass ratio of 5:5;
[0011] S3, add butyl acetate as a diluent, the mass of which is 10% to 15% of the mass of the resin matrix, and use a glass rod to fully stir to evenly disperse the components in the coating until no obvious particles can be seen in the coating with the naked eye;
[0012] S4, add 5% of KH560 and 7% of DOP to the resin matrix, and stir and disperse them evenly with a glass rod;
[0013] S5, placing the above coating in a cell crusher, inserting the horn in the cell crusher into the liquid by 10-20 mm, and using ultra-high frequency oscillation sound waves with a power of 25-100W and a pulse time of 1s / 2s-4s / 8s to perform cell crushing and enhanced dispersion treatment for 3-9 minutes;
[0014] S6. After strengthening treatment, a curing agent accounting for 25% of the mass of the resin matrix is added, and then a small amount of butyl acetate is added to adjust the viscosity of the coating to a suitable range;
[0015] S7. The above coating is applied to the tinplate substrate by glass rod scraping method, and the surface is dried at room temperature for 5 hours and then dried at 80°C for 3 hours to obtain a cell crushing-enhanced low-emissivity, low-gloss, and low-near-infrared reflectivity compatible coating.
[0016] Preferably, in step S1, the size of the tinplate plate is 12 cm×5 cm×0.2 mm.
[0017] Preferably, in step S2, the resin matrix is PU or epoxy resin, the solid content of the PU is 66.7%; the solid content of the epoxy resin is 66.7%.
[0018] Preferably, in step S6, the curing agent is a low molecular weight polyamide or a polyether polyol, the molecular weight of the low molecular weight polyamide or the polyether polyol is 750 to 1250, and the viscosity adjustment range is 15 to 20s using a four-cup viscosity measurement.
[0019] (III) Beneficial effects
[0020] Compared with the prior art, the present invention has the following beneficial effects: the present invention has a simple process, low production cost, and is easy to use. The obtained coating can be used on the surface of various aircraft, and can make it have a lower glossiness while achieving a good infrared and 1.06μm laser compatible stealth effect. It has broad application prospects in the field of infrared and multi-spectrum compatible stealth design and modification of various aircraft;
[0021] Compared with the traditional low infrared emissivity coating preparation process which requires three dispersion processes such as stirring, high-speed dispersion and grinding (sand grinding), only simple stirring and cell crushing and strengthening treatment processes are required. The preparation process is simpler, and the energy consumption and production cost are significantly reduced.
[0022] The coating prepared by the present invention has lower infrared emissivity, glossiness and 1.06 μm near-infrared reflectivity than the coating prepared by the traditional process, so that the obtained coating has better infrared and multi-spectrum compatible stealth effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the method steps of the present invention;
[0024] Figure 2 This is a real picture of the cell crushing enhanced low emissivity, low gloss and low near-infrared reflectivity compatible coating prepared by the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] See also Figure 1-2The embodiment of the present invention provides a technical solution: a method for preparing a low-emissivity and low-near-infrared reflectivity coating by a cell crushing method, the method steps comprising the following:
[0027] S1. Use a test-grade standard tinplate as the substrate, polish the substrate with 200-400 grit sandpaper to make it have a certain roughness, and wipe the substrate clean with disposable tissue dipped in alcohol for later use;
[0028] S2. Milling graphite and flaky Al powder for 30 to 60 minutes at a speed of 400 to 800 r / min using a high-energy planetary ball mill to obtain graphite-modified Al powder, and weighing appropriate amounts of resin matrix and graphite-modified Al powder in a clean disposable plastic cup in a mass ratio of 5:5;
[0029] S3, add butyl acetate as a diluent, the mass of which is 10% to 15% of the mass of the resin matrix, and use a glass rod to fully stir to evenly disperse the components in the coating until no obvious particles can be seen in the coating with the naked eye;
[0030] S4, add 5% of KH560 and 7% of DOP to the resin matrix, and stir and disperse them evenly with a glass rod;
[0031] S5, placing the above coating in a cell crusher, inserting the horn in the cell crusher into the liquid by 10-20 mm, and using ultra-high frequency oscillation sound waves with a power of 25-100W and a pulse time of 1s / 2s-4s / 8s to perform cell crushing and enhanced dispersion treatment for 3-9 minutes;
[0032] S6. After strengthening treatment, a curing agent accounting for 25% of the mass of the resin matrix is added, and then a small amount of butyl acetate is added to adjust the viscosity of the coating to a suitable range;
[0033] S7. The above coating is applied to the tinplate substrate by glass rod scraping method, and the surface is dried at room temperature for 5 hours and then dried at 80°C for 3 hours to obtain a cell crushing-enhanced low-emissivity, low-gloss, and low-near-infrared reflectivity compatible coating.
[0034] As a further improvement, in step S1, the size of the tinplate plate is 12 cm×5 cm×0.2 mm.
[0035] As a further improvement, in step S2, the resin matrix is PU or epoxy resin, the solid content of the PU is 66.7%; the solid content of the epoxy resin is 66.7%.
[0036] Further improved, in step S6, the curing agent is a low molecular weight polyamide or a polyether polyol, the molecular weight of the low molecular weight polyamide or the polyether polyol is 750 to 1250, and the viscosity adjustment range is 15 to 20s using a four-cup viscosity measurement.
[0037] Embodiment 1:
[0038] Use a high-energy planetary ball mill to ball-mill graphite and flaky Al powder for 60 minutes at a speed of 500r / min to obtain graphite-modified Al powder. Weigh an appropriate amount of PU and graphite-modified Al powder in a clean disposable plastic cup at a mass ratio of 5:5. Add butyl acetate as a diluent, the mass of which is 12% of the mass of the resin matrix, and use a glass rod to fully stir to evenly disperse the components in the coating until no obvious particles can be seen in the coating with the naked eye. Then add KH560 accounting for 5% of the mass of the resin matrix and DOP accounting for 7% of the mass of the resin matrix, and stir and disperse evenly with a glass rod. Place the above coating in a cell crusher, insert the amplitude rod in the cell crusher into the liquid 12mm, and use an ultra-high frequency oscillation sound wave with a power of 50w and a pulse time of 2s / 4s to enhance the dispersion treatment for 5min. After strengthening treatment, a low molecular weight polyamide curing agent accounting for 25% of the mass of the resin matrix is added, and then a small amount of butyl acetate is added to adjust the viscosity of the coating to an appropriate range (the viscosity is 17s measured by a coating cup). The above coating is applied to the tinplate substrate by glass rod scraping method, and the surface is dried at room temperature for 5 hours and dried at 80℃ for 3 hours to obtain a cell crushing strengthened low emissivity, low gloss, and low near-infrared reflectivity compatible coating. The infrared emissivity of the obtained coating is 0.275, the gloss is 5.5, the near-infrared reflectivity at 1.06μm is 35.6%, the adhesion is level 1, the flexibility is 2mm, and the impact strength is 50kg.cm.
[0039] Embodiment 2:
[0040] Use a high-energy planetary ball mill to ball-mill graphite and flaky Al powder for 50 minutes at a speed of 600r / min to obtain graphite-modified Al powder. Weigh an appropriate amount of epoxy resin and graphite-modified Al powder in a clean disposable plastic cup at a mass ratio of 5:5. Add butyl acetate as a diluent, the mass of which is 10% of the mass of the resin matrix, and use a glass rod to fully stir to evenly disperse the components in the coating until no obvious particles can be seen in the coating with the naked eye. Then add KH560 accounting for 5% of the mass of the resin matrix and DOP accounting for 7% of the mass of the resin matrix, and stir and disperse evenly with a glass rod. Place the above coating in a cell crusher, insert the amplitude rod in the cell crusher into the liquid 15mm, and use an ultra-high frequency oscillation sound wave with a power of 50w and a pulse time of 2s / 4s to enhance the dispersion treatment for 5min. After strengthening treatment, a polyether polyol curing agent accounting for 25% of the mass of the resin matrix is added, and then a small amount of butyl acetate is added to adjust the viscosity of the coating to an appropriate range (the viscosity is 15s when measured with a coating cup). The above coating is applied to the tinplate substrate by glass rod scraping method, and the surface is dried at room temperature for 5 hours and dried at 80℃ for 3 hours to obtain a cell crushing strengthened low emissivity, low gloss, and low near-infrared reflectivity compatible coating. The infrared emissivity of the obtained coating is 0.256, the gloss is 4.8, the near-infrared reflectivity at 1.06μm is 32.8%, the adhesion is level 1, the flexibility is 2mm, and the impact strength is 50kg.cm.
[0041] Embodiment 3:
[0042] Use a high-energy planetary ball mill to ball-mill graphite and flaky Al powder for 50 minutes at a speed of 600r / min to obtain graphite-modified Al powder. Weigh an appropriate amount of PU and graphite-modified Al powder in a clean disposable plastic cup at a mass ratio of 5:5. Add butyl acetate as a diluent, the mass of which is 15% of the mass of the resin matrix, and use a glass rod to fully stir to evenly disperse the components in the coating until no obvious particles can be seen in the coating with the naked eye. Then add KH560 accounting for 5% of the mass of the resin matrix and DOP accounting for 7% of the mass of the resin matrix, and stir and disperse evenly with a glass rod. Place the above coating in a cell crusher, insert the amplitude rod in the cell crusher into the liquid 18mm, and use an ultra-high frequency oscillation sound wave with a power of 75w and a pulse time of 3s / 6s for enhanced dispersion treatment for 3min. After strengthening treatment, a low molecular weight polyamide curing agent accounting for 25% of the mass of the resin matrix is added, and then a small amount of butyl acetate is added to adjust the viscosity of the coating to an appropriate range (the viscosity is 19s measured by a coating cup). The above coating is applied to the tinplate substrate by glass rod scraping method, and the surface is dried at room temperature for 5 hours and dried at 80℃ for 3 hours to obtain a cell crushing strengthened low emissivity, low gloss, and low near-infrared reflectivity compatible coating. The infrared emissivity of the obtained coating is 0.235, the gloss is 4.3, the near-infrared reflectivity at 1.06μm is 31.6%, the adhesion is level 1, the flexibility is 2mm, and the impact strength is 50kg.cm.
[0043] The coating prepared by the cell crushing strengthening method has an emissivity (8-14 μm) as low as 0.235 measured by an IR-2 dual-band infrared emissivity tester developed by the Shanghai Institute of Technical Physics, Chinese Academy of Sciences, which is 45.3% lower than the emissivity of the low infrared emissivity coating prepared by the traditional method; the gloss of the coating is measured as low as 4.3 by a JKGZ-60 mirror gloss meter produced by Tianjin Jingke Lian Material Testing Machine Co., Ltd., which is 52.5% lower than the gloss of the low infrared emissivity coating prepared by the traditional method; the reflectivity of the coating at a near-infrared wavelength of 1.06 μm is measured by a UV3600 ultraviolet-visible near-infrared spectrophotometer produced by Shimadzu Corporation of Japan, which is 54.6% lower than the 1.06 μm near-infrared reflectivity of the low infrared emissivity coating prepared by the traditional method; at the same time, the coating maintains excellent mechanical properties, with adhesion level 1, flexibility 2 mm, and impact strength 50 kg.cm.
[0044] Polyurethane (PU) or epoxy resin is used as adhesive, graphite-modified Al powder is used as functional filler, KH560 and DOP are used as modifiers, and butyl acetate is used as diluent.
[0045] Compared with low infrared emissivity coatings prepared by traditional methods, the emissivity of the coating prepared by the present invention is reduced by 45.3%, and the glossiness of the coating prepared by traditional methods is reduced by 52.5%; compared with low infrared emissivity coatings prepared by traditional methods, the 1.06μm near-infrared reflectivity is reduced by 54.6%; compared with traditional low infrared emissivity coating preparation methods, the preparation process of the present invention is simpler, and the energy consumption and production costs are significantly reduced.
[0046] The graphite-modified Al powder prepared by high-energy planetary ball milling can achieve the outstanding effects of flaky aluminum powder with low emissivity, low brightness and low near-infrared reflectivity.
[0047] On the basis of not changing the formula of low infrared emissivity coating, the cell crushing and strengthening treatment method is used to improve the coating performance, simplify the process steps and reduce the energy consumption of coating preparation, which has important practical significance for improving the performance of low infrared emissivity coating and reducing production costs.
[0048] The cell crushing enhancement method can use the ultra-high frequency oscillation of sound waves with a frequency higher than 20,000 Hz to disperse the large particles formed by the agglomeration of tiny pigment and filler particles suspended in the paint at the wave nodes due to the ultra-high frequency crushing oscillation, thereby improving their dispersion state in the paint, improving their dispersion uniformity, and preventing the agglomeration of pigment and filler particles in the paint.
[0049] The cell crushing enhanced dispersion treatment is highly efficient. By effectively regulating the oscillation power, oscillation time, and pulse time (the cycle time ratio of the oscillation wave on and off), the dispersion state of various color and filler particles in the coating can be significantly improved, which is expected to significantly improve the comprehensive performance of the low infrared emissivity coating.
[0050] The invention has a simple process, low production cost and is easy to use. The obtained coating can be used for the surface of various aircraft, making it have a lower glossiness while achieving good infrared and laser compatible stealth effects. It has broad application prospects in the field of infrared and multi-spectrum compatible stealth design and modification of various aircraft.
[0051] Compared with the traditional low infrared emissivity coating preparation process which requires three dispersion processes such as stirring, high-speed dispersion and grinding (sand grinding), only simple stirring and cell crushing and strengthening treatment processes are required. The preparation process is simpler, and the energy consumption and production cost are significantly reduced.
[0052] The coating prepared by the present invention has lower infrared emissivity, glossiness and 1.06 μm near-infrared low reflectivity compared to the coating prepared by the traditional process, so that the obtained coating has better infrared and multi-spectrum compatible stealth effect.
[0053] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.
[0054] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a low-emissivity and low near-infrared reflectivity coating by a cell crushing method, characterized in that: The method steps include the following: S1. Use a test-grade standard tinplate as the substrate, polish the substrate with 200-400 grit sandpaper to make it have a certain roughness, and wipe the substrate clean with disposable tissue dipped in alcohol for later use; S2. Milling graphite and flaky Al powder for 30 to 60 minutes at a speed of 400 to 800 r / min using a high-energy planetary ball mill to obtain graphite-modified Al powder, and weighing appropriate amounts of resin matrix and graphite-modified Al powder in a clean disposable plastic cup in a mass ratio of 5:5; S3, add butyl acetate as a diluent, the mass of which is 10% to 15% of the mass of the resin matrix, and use a glass rod to fully stir to evenly disperse the components in the coating until no obvious particles can be seen in the coating with the naked eye; S4, add 5% of KH560 and 7% of DOP to the resin matrix, and stir and disperse them evenly with a glass rod; S5, placing the above coating in a cell crusher, inserting the horn in the cell crusher into the liquid by 10-20 mm, and using ultra-high frequency oscillation sound waves with a power of 25-100W and a pulse time of 1s / 2s-4s / 8s to perform cell crushing and enhanced dispersion treatment for 3-9 minutes; S6. After strengthening treatment, a curing agent accounting for 25% of the mass of the resin matrix is added, and then a small amount of butyl acetate is added to adjust the viscosity of the coating to a suitable range; S7. The above coating is applied to the tinplate substrate by glass rod scraping method, and the surface is dried at room temperature for 5 hours and then dried at 80°C for 3 hours to obtain a cell crushing-enhanced low-emissivity, low-gloss, and low-near-infrared reflectivity compatible coating.
2. The method for preparing a low-emissivity and low near-infrared reflectivity coating by a cell crushing method according to claim 1, characterized in that: In step S1, the size of the tinplate plate is 12 cm×5 cm×0.2 mm.
3. The method for preparing a low-emissivity and low near-infrared reflectivity coating by a cell crushing method according to claim 1, characterized in that: In step S2, the resin matrix is PU or epoxy resin, the solid content of the PU is 66.7%; the solid content of the epoxy resin is 66.7%.
4. The method for preparing a low-emissivity and low near-infrared reflectivity coating by a cell crushing method according to claim 1, characterized in that: In step S6, the curing agent is a low molecular weight polyamide or a polyether polyol, the molecular weight of the low molecular weight polyamide or the polyether polyol is 750 to 1250, and the viscosity adjustment range is 15 to 20s measured by a four-cup coating.
Citation Information
Patent Citations
Preparation method of visible light full-waveband multilayer antireflection coating
CN102838889A
Method for preparing infrared radiation high-heat-dissipation coating on surface of chemical pump shell
CN109554034A
Black shading conductive coating and preparation method thereof
CN113337198A
Infrared low-emissivity coating without metal filler
CN114106654A
Preparation method of coating with ultralow infrared emissivity
CN115926571A