Waste plastic pyrolysis cracking pretreatment method and reaction device, waste plastic pyrolysis cracking method and processing system
Through rapid liquefaction and plastic reduction and viscosity reduction treatment of twin-screw heating equipment, combined with wax oil distillate circulation technology, the problem of polyvinyl chloride decomposition and slow heat transfer in waste plastic pyrolysis treatment is solved, and high-efficiency large-scale waste plastics are achieved Resource utilization.
Patent Information
- Application Number
- CN202310632258.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art has problems in the pyrolysis treatment of waste plastics, which are difficult to decompose polyvinyl chloride, slow heat transfer, and high coke rate and device blockage, and the treatment scale is small and cannot meet the needs of large-scale recycling.
The double-screw heating and conveying equipment is used for rapid liquefaction treatment, and the heating furnace of the front section coarse furnace and the back section fine furnace tube are used for plastic reduction and viscosity reduction treatment, which improves the temperature and fluidity of waste plastics, and uses wax in the pyrolysis reaction. The oil fraction acts as a circulating oil to regulate the product structure and reduce coke generation.
It realizes high-efficiency liquid yield and low coking rate of waste plastics, large-scale continuous recycling, reduces processing costs, and adapts to modern large-scale recycling needs.
Smart Images

Figure CN119060751A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of waste plastic resource recycling, and in particular to a heating method and an application system for rapid liquefaction, pyrolysis and cracking of waste plastic. Background Art
[0002] With the advancement of science and technology and industrial development, plastics are widely used as packaging materials in people's daily lives. Used waste plastics cannot be decomposed by themselves in nature. Only a few types of waste plastics can be reprocessed and reused through specific recycling channels. A large amount of waste plastics enters landfills in the form of domestic garbage. Since waste plastics are not easy to decompose, they occupy a lot of space. In recent years, the amount of waste plastics has increased, and it has become an urgent task to recycle waste plastics quickly and greenly.
[0003] The simplest chemical method to deal with waste plastics is direct incineration, but direct incineration will produce toxic gases that are harmful to the human body and cause secondary environmental pollution. Waste plastic oil technology is to crack waste plastics under anaerobic or anoxic conditions by heating or catalyst conditions to crack polymers into low molecular weight substances to obtain gasoline, kerosene, diesel fractions and some pyrolysis gases. On the one hand, waste plastic oil technology alleviates the pollution problem caused by waste plastics, and on the other hand, it realizes the recycling of waste plastics, which is an important direction for the resource treatment of waste plastics.
[0004] At present, waste plastic oil recovery technology mainly includes waste plastic thermal cracking, catalytic thermal cracking and thermal cracking catalytic modification technology. The thermal cracking method has the advantages of simple process, relatively less equipment investment, no catalyst required, and short reaction process, making the thermal cracking method the lowest unit oil cost compared to the other two technologies. General waste plastics in domestic garbage undergo high-temperature thermal cracking reaction between 380 and 500°C, with a fast cracking speed and a relatively simple product composition, which can be used as oil products or chemical raw materials.
[0005] 201811473414.0 discloses a waste plastic continuous thermal cracking system and a thermal cracking method thereof, the system includes a loading device, a feeding device, a thermal cracking reactor and a slag discharge device connected in sequence. Since plastic is a macromolecular polymer, a non-Newtonian fluid is formed during the heating process, and a screw propeller is used. The plastic liquefaction process in this process is subjected to uneven heating, which is prone to coking and fouling. ZL201310540472.1 discloses a coking method for producing fuel oil from waste plastics, the method is to preheat high aromatic components and waste plastics or plastic oil in a raw material buffer tank, enter a tubular heating furnace for heating, and then spray into a delayed coking tower for coking reaction. The waste plastics mentioned in this method are one or more of polyethylene, polypropylene and polystyrene, and do not contain polyvinyl chloride, so it is impossible to process waste plastic raw materials mixed with polyvinyl chloride. Patent 202010868490.2 discloses a method for co-converting waste plastics in a delayed coker unit, which converts waste plastics together with petroleum residue raw materials, wherein the waste plastics are selected from polyethylene, polypropylene, polystyrene, PET and multi-layer plastics with added metals, and also do not include waste plastics of polyvinyl chloride. Waste plastics form high-viscosity polymer melts during the melting process, which have a density difference with hydrocarbon raw materials. Therefore, the mixed fluid of hydrocarbon and polymer melts can cause problems such as blockage and coking of delayed coking heating furnace tubes. Summary of the invention
[0006] One of the technical problems solved by the present invention is to provide a pretreatment method and system for pyrolysis and cracking of waste plastics.
[0007] One of the technical problems solved by the present invention is to provide a method and system for pyrolysis and cracking of waste plastics, which can effectively realize the resource-based, large-scale and continuous utilization of waste plastics and reduce the generation of coke.
[0008] In a first aspect, the present invention provides a method for pre-treating waste plastic by pyrolysis and cracking, comprising:
[0009] S1, allowing the waste plastic to be processed to enter the waste plastic liquefaction unit for liquefaction treatment to obtain liquefied waste plastic, wherein the waste plastic liquefaction unit adopts a first twin-screw heating and conveying device;
[0010] S2, the liquefied waste plastic enters the plastic reduction and viscosity reduction heating unit for plastic reduction and viscosity reduction cracking treatment to obtain high-temperature liquefied waste plastic oil and dry gas after plastic reduction and viscosity reduction cracking; the plastic reduction and viscosity reduction heating unit adopts a heating furnace, and its heating furnace tube consists of a front section thick furnace tube and a rear section thin furnace tube.
[0011] In step S1, optionally, the operating conditions of the liquefaction treatment are: the outlet temperature of the liquefied waste plastic is 330-380°C, preferably 340-360°C; the residence time is 1-20 min, preferably 5-15 min.
[0012] In step S2, optionally, the inner diameter ratio of the front thick furnace tube and the rear thin furnace tube is 2-4:1, preferably 2-3:1; the length ratio of the front thick furnace tube and the rear thin furnace tube is 0.1-0.6:1, preferably 0.2-0.6:1.
[0013] In a second aspect, the present invention provides a waste plastic pyrolysis and cracking pretreatment reaction device, comprising a first twin-screw heating and conveying device and a heating furnace connected thereto; the furnace tube of the heating furnace is composed of a front section thick furnace tube and a rear section thin furnace tube connected together.
[0014] Optionally, the inner diameter ratio of the front thick furnace tube and the rear thin furnace tube is 2-4:1, preferably 2-3:1; the length ratio of the front thick furnace tube and the rear thin furnace tube is 0.1-0.6:1, preferably 0.2-0.6:1.
[0015] In a third aspect, the present invention provides a method for pyrolysis and cracking of waste plastics, comprising any of the above-mentioned pretreatment methods for pyrolysis and cracking of waste plastics, and,
[0016] S3, the high temperature liquefied waste plastic oil enters the pyrolysis reaction unit for pyrolysis reaction to obtain pyrolysis products and coke;
[0017] S4. The pyrolysis products enter a separation unit for separation to obtain dry gas, liquefied gas, gasoline fraction, diesel fraction and wax oil fraction.
[0018] Optionally, in step S3, the operating conditions of the pyrolysis reaction include: the pyrolysis tower top pressure is 0.05-0.6MPa, preferably 0.1-0.3MPa; the pyrolysis reaction temperature is 450-580°C, preferably 480-550°C, and the pyrolysis tower operation cycle is 1h-500h, preferably 10h-240h. The pyrolysis tower operation cycle refers to the single tower operation time of the pyrolysis tower, or the pyrolysis tower switching operation time.
[0019] In a fourth aspect, the present invention provides a waste plastic pyrolysis and cracking processing system, comprising a waste plastic liquefaction unit, a plastic reduction and viscosity reduction heating unit, a pyrolysis reaction unit and a separation unit; the waste plastic liquefaction unit comprises an inlet for waste plastic to be processed and an outlet for liquefied waste plastic, and the waste plastic liquefaction unit is configured to perform preliminary liquefaction treatment on the waste plastic to be processed; the plastic reduction and viscosity reduction heating unit comprises a heating inlet and a heating outlet, the heating inlet is connected to the outlet for liquefied waste plastic, the furnace pipe of the heating furnace of the plastic reduction and viscosity reduction heating unit is composed of a front section thick furnace pipe and a rear section thin furnace pipe connected, and the plastic reduction and viscosity reduction heating unit is connected to the outlet for liquefied waste plastic. The unit is configured to reduce the plasticity and viscosity of the initially liquefied waste plastics and perform a heating treatment; the pyrolysis reaction unit includes a pyrolysis reactant inlet and a pyrolysis product outlet, the pyrolysis reactant inlet is connected to the outlet of the material mixing unit, and the pyrolysis reaction unit is configured to perform a pyrolysis reaction treatment on the high-temperature liquefied waste plastics; the separation unit includes a separation inlet, a dry gas outlet, a liquefied gas outlet, a gasoline fraction outlet, a diesel fraction outlet and a wax oil fraction outlet; the separation inlet is connected to the pyrolysis product outlet of the pyrolysis reaction unit, and the separation unit is configured to perform separation treatment on the pyrolysis products.
[0020] Compared with the prior art, the present invention provides a pretreatment method and reaction device for pyrolysis and cracking of waste plastics, as well as a method and processing system for pyrolysis and cracking of waste plastics for plastic reduction and viscosity reduction. The present invention directly enters the plastic reduction and viscosity reduction heating unit for treatment by rapidly liquefying the waste plastics to be treated. The front-end thick furnace tube is used in the plastic reduction and viscosity reduction heating unit to extend the residence time, and the rear-end thin furnace tube is used to fully increase the temperature of the liquefied waste plastics to quickly obtain high-temperature waste plastic oil. The method has a simple process, reduces the difficulty of plastic reduction and viscosity reduction operation, transports the high-temperature liquefied waste plastics to the pyrolysis tower for pyrolysis reaction, realizes the resource utilization of waste plastics, and reduces the generation of coke. Through the waste plastic processing method provided by the present invention, subsequent cracking recovery can be centrally processed, it is easy to expand the production scale, and reduce the processing cost; the process flow is simple, the equipment investment is relatively small, so that waste plastics can be recycled on a large scale, continuously, and greenly.
[0021] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0023] Figure 1 The present invention is a schematic flow chart of an implementation method of a pyrolysis and cracking pretreatment method for waste plastics.
[0024] Figure 2The figure is a schematic flow chart of a second embodiment of the method for pre-treating waste plastics by pyrolysis and cracking.
[0025] Figure 3 The present invention is a schematic flow chart of one embodiment of a method for pyrolysis and cracking of waste plastics.
[0026] in:
[0027] 1- Waste plastic storage tank 2- Melting dechlorination unit 3- Waste plastic liquefaction unit
[0028] 4-plastic reduction and viscosity reduction heating unit 5-pyrolysis reaction unit 6-separation unit 7-hydrogen chloride absorption unit 12-diesel fraction outlet 13-liquefied gas gasoline fraction outlet
[0029] Port 14 - gas outlet 15 - wax oil fraction outlet 18, 19 - circulating oil inlet 21 - front section thick furnace tube 22 - rear section thin furnace tube 9-11, 16, 17, 20 - pipeline DETAILED DESCRIPTION
[0030] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0031] In a first aspect, the present invention provides a method for pre-treating waste plastic by pyrolysis and cracking, comprising:
[0032] S1, allowing the waste plastic to be processed to enter the waste plastic liquefaction unit for liquefaction treatment to obtain liquefied waste plastic, wherein the waste plastic liquefaction unit adopts a first screw-type heating and conveying device;
[0033] S2, the liquefied waste plastic enters the plastic reduction and viscosity reduction heating unit for plastic reduction and viscosity reduction cracking treatment to obtain high-temperature liquefied waste plastic oil and non-condensable steam after plastic reduction and viscosity reduction cracking; the plastic reduction and viscosity reduction heating unit adopts a heating furnace, and its heating furnace tube consists of a front section thick furnace tube and a rear section thin furnace tube.
[0034] In step S1, optionally, the operating conditions of the liquefaction treatment in the first screw-type heating and conveying device are: the outlet temperature of the liquefied waste plastic is 330-380°C, preferably 340-360°C; the residence time is 1-20 minutes, preferably 5-15 minutes. The present invention has no restriction on the feed rate of the first screw-type heating and conveying device, and the feed rate of the screw-type heating and conveying device is related to the processing capacity of the device; for a certain processing capacity, one screw-type heating and conveying device can be used, or multiple screw-type heating and conveying devices can be used in parallel.
[0035] In step S2, optionally, the inner diameter ratio of the front thick furnace tube and the rear thin furnace tube is 2 to 4:1, preferably 2 to 3:1; the length ratio of the front thick furnace tube and the rear thin furnace tube is 0.1 to 0.6:1, preferably 0.2 to 0.6:1. Optionally, the volume ratio of the front thick furnace tube and the rear thin furnace tube is 5 to 20:1, preferably 8 to 15:1.
[0036] In the method provided by the present invention, the first screw-type heating and conveying device is directly connected to the heating furnace. The heating furnace tube is a structure with a thick front and a thin rear. The waste plastic oil stays in the front furnace tube for a long time and mainly undergoes plastic reduction, viscosity reduction and cracking reactions; the rear furnace tube has a thinner diameter and is used to increase the temperature of the plastic reduction, viscosity reduction and liquefaction of the waste plastic.
[0037] Optionally, the operating conditions of the front-stage rough furnace tube are: reaction temperature is 360-420° C., preferably 380-400° C.; residence time is 10-60 min, preferably 15-30 min.
[0038] Optionally, the operating conditions of the rear-stage thin furnace tubes are: the outlet temperature of the heating furnace is 480°C to 550°C, preferably 480°C to 540°C; optionally, water vapor is injected into the rear-stage thin furnace tubes to accelerate the material flow rate and prevent coking of the heating furnace tubes, and the steam injection amount is 0 to 5% by weight, preferably 0.5 to 3% by weight.
[0039] The front section furnace pipe of the heating furnace is used as the plastic reduction and viscosity reduction part, and the heating method can be heat exchange or other conventional methods. The rear section furnace pipe of the heating furnace has a thinner pipe diameter, which is used to increase the temperature of the mucilaginous waste plastics, and the heating method can be heat exchange or other conventional methods. The front section furnace pipe and the rear section furnace pipe can be connected directly or through a transition connection of a tapered diameter reducing section.
[0040] In a second aspect, the present invention provides a waste plastic pyrolysis and cracking pretreatment reaction device, comprising a first screw-type heating and conveying device and a heating furnace connected thereto; the furnace tube of the heating furnace is composed of a front section thick furnace tube and a rear section thin furnace tube connected together.
[0041] Optionally, the inner diameter ratio of the front furnace tube and the rear furnace tube is 2 to 4:1, preferably 2 to 3:1; the length ratio is 0.1 to 0.6:1, preferably 0.2 to 0.6:1. The front thick furnace tube and the rear thin furnace tube can be connected directly or through a transition connection of a conical reducer. Optionally, the first screw heating and conveying device is a single screw heating and conveying device or a twin screw heating and conveying device, preferably a twin screw heating and conveying device.
[0042] In a third aspect, the present invention provides a method for pyrolysis and cracking of waste plastics, comprising any of the above-mentioned pretreatment methods for pyrolysis and cracking of waste plastics, and,
[0043] S3, the high temperature liquefied waste plastic oil enters the pyrolysis reaction unit for pyrolysis reaction to obtain pyrolysis products and coke;
[0044] S4. The pyrolysis products enter a separation unit for separation to obtain dry gas, liquefied gas, gasoline fraction, diesel fraction and wax oil fraction.
[0045] Optionally, in step S3, the operating conditions of the pyrolysis reaction include: the top pressure of the pyrolysis tower is 0.05-0.6MPa, preferably 0.1-0.3MPa; the pyrolysis reaction temperature is 450-580°C, preferably 480-550°C; the pyrolysis tower operation cycle is 1h-500h, preferably 10h-240h. The pyrolysis tower operation cycle refers to the single tower operation time of the pyrolysis tower, or the pyrolysis tower switching operation time.
[0046] Optionally, the wax oil fraction is returned to step S2 for recycling, and the recycled wax oil fraction is added to the starting end of the front thick furnace tube, and the weight ratio of the recycled wax oil fraction to the liquefied waste plastic is 0.2 to 5.0:1, preferably 0.2 to 2:1.
[0047] The wax oil fraction is a fraction with a distillation range of more than 350° C. obtained by separation of the separation unit or a fraction with a distillation range of more than 350° C. obtained by other processes.
[0048] When the front thick furnace tube is directly connected to the rear thin furnace tube, circulating oil is added from the starting end of the front thick furnace tube and at the same time, circulating oil is added from the end of the front thick furnace tube to overcome the stagnant flow area of the fluid in the front thick furnace tube of the heating furnace. When the front thick furnace tube is connected to the rear thin furnace tube using a reducing section, circulating oil may not be added to the end of the front thick furnace tube.
[0049] Through the above technical scheme, the present invention provides a waste plastic pyrolysis cracking method and processing system. In the preferred technical scheme, adding wax oil fraction as circulating oil can adjust the product structure and can also carry more heat into the reactor.
[0050] Optionally, the method provided by the present invention further comprises:
[0051] S0, the chlorine-containing waste plastic raw material enters the melting dechlorination unit for hot melt dechlorination treatment to obtain dry gas containing hydrogen chloride and dechlorinated waste plastic material; the dechlorinated waste plastic material enters the waste plastic liquefaction unit of S1; or the dechlorinated waste plastic material is cooled and crushed in turn to obtain dechlorinated waste plastic particles, and the dechlorinated waste plastic particles enter the waste plastic liquefaction unit of S1.
[0052] Optionally, the waste plastic melting dechlorination unit comprises a second screw heating and conveying device and a vacuum device connected to the second screw heating and conveying device; preferably, the second screw heating and conveying device is selected from a twin-screw or single-screw conveying device;
[0053] In the waste plastic melting dechlorination unit, the waste plastic raw material is first heated and dehydrated, and then subjected to hot melt dechlorination treatment. The process conditions of the hot melt dechlorination treatment include: a feed rate of 5 to 5000 kg / h, preferably 100 to 4000 kg / h; an outlet temperature of 150 to 370°C, preferably 300 to 330°C, a reaction time of 0.1 to 0.5 h, preferably 0.1 to 0.3 h; a vacuum degree of the waste plastic melting dechlorination unit of 50 to 300 mmHg, preferably 50 to 150 mmHg; preferably, the particle size of the dechlorinated waste plastic particles obtained by the crushing treatment is 100 to 2000 μm.
[0054] Optionally, step S0 further comprises: allowing the obtained dry gas containing hydrogen chloride to enter a hydrogen chloride absorption unit, contacting with a hydrogen chloride absorbent to perform hydrogen chloride absorption treatment, and obtaining a chlorine-containing absorbent and a dechlorinated dry gas; optionally, allowing the dry gas containing hydrogen chloride to enter the hydrogen chloride absorption unit under the action of a vacuum system; wherein the hydrogen chloride absorbent is water or an alkali solution with a pH greater than 7; optionally, the alkali solution comprises one or more of a sodium hydroxide solution, a potassium hydroxide solution, a calcium hydroxide solution, a sodium bicarbonate solution, a sodium carbonate solution and an ammonia solution.
[0055] In the preferred technical solution, the chlorine-containing waste plastics are first subjected to melting and dechlorination treatment, the waste plastics in the landfill can be dehydrated, dechlorinated and reduced in situ, and dechlorinated waste plastic oil is obtained in the subsequent step.
[0056] In the method provided by the present invention, the waste plastics to be processed include one or more of low-density polyethylene (LDPE), high-density polyethylene (HDPE), polystyrene (PS), polypropylene (PP), polyethylene terephthalate (PET) and polyvinyl chloride (PVC);
[0057] Optionally, the PVC content in the waste plastic to be processed is less than 10 wt %; the ash content in the waste plastic to be processed is 1 to 40 wt %, preferably 3 to 30 wt %. The waste plastic raw material in the present invention can be directly waste plastic in landfill.
[0058] In a fourth aspect, the present invention provides a waste plastic pyrolysis and cracking processing system, comprising a waste plastic liquefaction unit, a plastic reduction and viscosity reduction heating unit, a pyrolysis reaction unit and a separation unit; the waste plastic liquefaction unit comprises an inlet for waste plastic to be processed and an outlet for liquefied waste plastic, and the waste plastic liquefaction unit is configured to perform preliminary liquefaction treatment on the waste plastic to be processed; the plastic reduction and viscosity reduction heating unit comprises a heating inlet and a heating outlet, the heating inlet is connected to the outlet for liquefied waste plastic, the furnace pipe of the heating furnace of the plastic reduction and viscosity reduction heating unit is composed of a front section thick furnace pipe and a rear section thin furnace pipe connected, and the plastic reduction and viscosity reduction heating unit The element is configured to reduce plasticity, viscosity, crack and heat the preliminary liquefied waste plastics; the pyrolysis reaction unit includes a pyrolysis reactant inlet and a pyrolysis product outlet, the pyrolysis reactant inlet is connected to the material mixing unit outlet, and the pyrolysis reaction unit is configured to perform pyrolysis reaction treatment on the high-temperature liquefied waste plastics; the separation unit includes a separation inlet, a dry gas outlet, a liquefied gas outlet, a gasoline fraction outlet, a diesel fraction outlet and a wax oil fraction outlet; the separation inlet is connected to the pyrolysis product outlet of the pyrolysis reaction unit, and the separation unit is configured to separate the pyrolysis products.
[0059] Optionally, in the heating furnace, the inner diameter ratio of the front thick furnace tube and the rear thin furnace tube is 2-4:1, preferably 2-3:1; the length ratio of the front thick furnace tube and the rear thin furnace tube is 0.1-0.6:1, preferably 0.2-0.6:1.
[0060] Optionally, the system also includes a waste plastic melting dechlorination unit and a hydrogen chloride absorption unit; the waste plastic melting dechlorination unit includes an inlet for chlorine-containing waste plastic raw materials, an outlet for gaseous materials containing hydrogen chloride and an outlet for liquid materials of dechlorinated waste plastics, and the waste plastic melting dechlorination unit is configured to perform hot melt dechlorination treatment on the chlorine-containing waste plastic raw materials; the outlet for liquid materials of dechlorinated waste plastics is connected to an inlet for waste plastics to be treated of the waste plastic liquefaction unit; the hydrogen chloride absorption unit includes an inlet for gaseous materials containing hydrogen chloride, a hydrogen chloride absorbent and an outlet for dechlorinated dry gas; the inlet for gaseous materials containing hydrogen chloride is connected to the outlet for gaseous materials containing hydrogen chloride of the waste plastic melting dechlorination unit.
[0061] Preferably, the waste plastic liquefaction includes a heating liquefaction conveying device; optionally, the heating liquefaction conveying device includes a first screw heating conveying device; preferably, the first screw heating conveying device is selected from a twin-screw or single-screw heating conveying device with heating; preferably, the waste plastic melting and dechlorination unit includes a second screw heating conveying device and a vacuum device connected to the second screw heating conveying device; preferably, the second screw heating conveying device is selected from a twin-screw conveying device; preferably, the plastic reduction and viscosity reduction heating unit includes a circulating oil inlet; the circulating oil inlet is connected to the wax oil fraction outlet of the separation unit; optionally, the waste plastic melting and dechlorination unit also includes a non-condensable steam outlet.
[0062] In one embodiment, the waste plastic pyrolysis cracking processing system comprises a first twin-screw heating and conveying device, a heating furnace, a pyrolysis tower and a fractionation tower connected in sequence; the furnace tube of the heating furnace is composed of a front thick furnace tube and a rear thin furnace tube. Optionally, it also comprises a second screw heating and conveying device and a vacuum pumping device, wherein the gas phase outlet of the second screw heating and conveying device is connected to the vacuum pumping device, and the material outlet of the second screw heating and conveying device is connected to the material inlet of the first twin-screw heating device.
[0063] In the waste plastic pyrolysis cracking processing method provided by the present invention, in one embodiment, in step S1, the waste plastic liquefaction unit uses a rapid heating liquefaction conveying device to perform the liquefaction treatment; optionally, the rapid heating liquefaction conveying device includes a first screw heating conveying device; preferably, the first screw heating conveying device is selected from a twin-screw or single-screw heating conveying device with heating. The rapid heating liquefaction conveying device used in the present invention is conducive to the rapid liquefaction treatment of solid waste plastics.
[0064] In one embodiment, the waste plastic liquefaction unit described in step S1 adopts a first twin-screw heating and conveying device; preferably, the process conditions of the liquefaction treatment include: an outlet temperature of 330 to 380°C, preferably 340 to 360°C; a residence time of 1 to 20 minutes, preferably 5 to 15 minutes.
[0065] In a preferred embodiment, before step S1, the method further comprises:
[0066] The chlorine-containing waste plastic raw material enters the waste plastic melting and dechlorination unit for hot melt dechlorination treatment to obtain a gas phase material containing hydrogen chloride and a dechlorinated waste plastic material;
[0067] allowing the dechlorinated waste plastic material to enter the waste plastic liquefaction unit; or
[0068] The dechlorinated waste plastic material is subjected to cooling treatment and crushing treatment in sequence to obtain dechlorinated waste plastic particles; and the dechlorinated waste plastic particles are allowed to enter the waste plastic liquefaction unit.
[0069] The waste plastic melting dechlorination unit comprises a second screw heating and conveying device and a vacuum device connected to the second screw heating and conveying device; preferably, the second screw heating and conveying device is selected from a twin-screw or single-screw conveying device;
[0070] In the present invention, the hot melt dechlorination step and the waste plastic liquefaction step can use the same rapid heating liquefaction conveying equipment, or each can use a rapid heating liquefaction conveying equipment; for example, the rapid heating liquefaction conveying equipment is a screw-type heating conveying equipment with heating, etc.
[0071] In a preferred embodiment, the method further comprises: allowing the hydrogen chloride-containing gas to enter a hydrogen chloride absorption unit, contacting with a hydrogen chloride absorbent to perform hydrogen chloride absorption treatment, and obtaining a chlorine-containing absorbent and dechlorinated dry gas; optionally, allowing the hydrogen chloride-containing gas to enter the hydrogen chloride absorption unit under the action of a vacuum system.
[0072] When treating chlorine-containing waste plastics, the present invention decomposes the chlorine of the chlorine-containing waste plastic PVC into the gas phase through the waste plastic melting dechlorination unit, and can use a vacuum system to quickly separate hydrogen chloride, avoid secondary reaction of hydrogen chloride, improve the dechlorination efficiency of the waste plastics, and reduce the anti-corrosion pressure of subsequent equipment.
[0073] In a preferred embodiment, the method further comprises:
[0074] Returning at least part of the wax oil fraction or other process wax oil fraction from the separation unit to the plastic reduction and viscosity reduction heating unit for recycling;
[0075] Preferably, the fraction separated by the separation unit with a distillation range of more than 350°C is used as the wax oil fraction. Processing according to this embodiment can further improve the utilization efficiency of waste plastic resources; and introducing the wax oil fraction into the plastic reduction and viscosity reduction heating unit is also beneficial to the plastic reduction and viscosity reduction cracking treatment of waste plastics.
[0076] In the present invention, the pyrolysis reaction unit may include a plurality of pyrolysis towers arranged in parallel.
[0077] The beneficial effect of the waste plastic thermal cracking method provided by the present invention is to overcome the technical problems existing in the field of waste plastic thermal decomposition treatment. The inventor found in the research process that one of the technical problems existing in the prior art is that the polyvinyl chloride in the waste plastic is decomposed into HCl by heat, which can quickly react with the double bonds in the raw materials to form chlorinated hydrocarbons, making it difficult for the traditional reaction device to efficiently remove chlorine from the waste plastic. In response to the first technical problem, the present invention uses special equipment to quickly heat the polyvinyl chloride to decompose it, and uses a vacuum method to quickly separate the decomposed HCl from the reactor to improve the dechlorination efficiency. The second technical problem existing in the prior art overcomes: waste plastics are high molecular polymers. Due to their huge molecular weight and solid state, the heat transfer inside the plastic is very slow. The traditional heating method will cause the plastic to be overheated and cracked on the outside, while the inside of the plastic is still solid, resulting in a high pyrolysis coke rate and a high gas yield of the waste plastics. In response to the second technical problem, a special device is used to increase the heating area through strong extrusion and stirring to quickly heat the waste plastics to a flowable liquid state, and then a heating furnace with a thick furnace tube in the front section and a thin furnace tube in the rear section is used to directly reduce plasticity, viscosity, and temperature, and pyrolysis the liquid waste plastics to obtain a higher liquid yield and a lower coking rate. The third technical problem overcomes: the density of waste plastics is low, and the rate at which waste plastics enter the reaction device is low. The processing scale of the existing technology is small and cannot meet the needs of modern large-scale recycling. In response to the third technical problem, after the waste plastics are liquefied by the method provided by the present invention, the transportation density of the raw materials is greatly increased compared with that of solid waste plastics, so that not only the large-scale processing of waste plastics can be achieved, but also the continuous pyrolysis recovery of waste plastics can be achieved.
[0078] The technical solution of the present invention is described in detail below with reference to the accompanying drawings, but the present invention is not limited thereto in any way.
[0079] Attached Figure 1 The schematic diagram of the first embodiment of the pyrolysis and cracking pretreatment method for waste plastics is shown in the figure. Figure 1 As shown, the waste plastic to be treated enters the waste plastic liquefaction unit 3 for liquefaction treatment to obtain liquefied waste plastic; the liquefied waste plastic enters the plastic reduction and viscosity reduction heating unit 4 for plastic reduction and viscosity reduction cracking treatment to obtain high-temperature liquefied waste plastic oil and non-condensable gas after plastic reduction and viscosity reduction cracking. Specifically, the pretreatment device for pyrolysis and cracking of waste plastics includes a first screw-type heating and conveying device and a heating furnace connected thereto; wherein the heating furnace tube is composed of a front-stage thick furnace tube 21 and a rear-stage thin furnace tube 22. The front-stage thick furnace tube and the rear-stage thin furnace tube are directly connected, and the circulating oil can be supplemented through the circulating oil inlet 18 at the starting end of the front-stage thick furnace tube, and the circulating oil can be supplemented through the circulating oil inlet 19 at the end of the front-stage thick furnace tube.
[0080] Attached Figure 2 The figure is a schematic diagram of the second embodiment of the method for pre-treating waste plastic by pyrolysis and cracking. Figure 1The difference is that the front thick furnace tube and the rear thin furnace tube in the heating furnace are connected via a reducing section, and the circulating oil only needs to be replenished through the circulating oil inlet 18 at the starting end of the front thick furnace tube.
[0081] Attached Figure 3 The following is a schematic diagram of the process of pyrolysis and cracking of waste plastics. Figure 3 As shown, the waste plastic pyrolysis cracking processing system includes: a melting dechlorination unit 2, a waste plastic liquefaction unit 3, a plastic reduction and viscosity reduction heating unit 4, a pyrolysis reaction unit 5 and a separation unit 6 which are connected in sequence; wherein the gas phase outlet of the melting dechlorination unit is connected to the hydrogen chloride absorption unit 7. The separation unit 6 includes a separation inlet, a gas outlet 14, a liquefied gas gasoline fraction outlet 13, a diesel fraction outlet 12 and a wax oil fraction outlet 15; the wax oil fraction outlet 15 of the separation unit is connected to the circulating oil inlet 18 of the plastic reduction and viscosity reduction heating unit.
[0082] A preferred embodiment of the process flow of the waste plastic pyrolysis cracking method provided by the present invention includes: Figure 3 As shown, the waste plastics stored in the waste plastic storage tank 1 enter the melting dechlorination unit 2, and after dehydration, deairing and dechlorination, a gaseous material containing hydrogen chloride and a dechlorinated waste plastic material are obtained. The air and water vapor are first discharged from the pipeline 17 through the vacuum system, and then the gaseous material containing hydrogen chloride is drawn into the hydrogen chloride absorption unit 7 through the vacuum system to contact with the hydrogen chloride absorbent for hydrogen chloride absorption treatment, thereby obtaining a chlorine-containing absorbent and dechlorinated dry gas, and a small amount of non-condensable gas is discharged through the pipeline 20. The dechlorinated waste plastic liquid phase material from the melting dechlorination unit 2 can directly enter the waste plastic liquefaction unit 3. The waste plastic liquefaction unit adopts a first screw-type heating and conveying device. After extrusion and heating by the first screw-type heating and conveying device, molten liquefied waste plastic is obtained; the liquefied waste plastic is sent to the plastic reduction and viscosity reduction heating unit 4 through a pipeline 9. The plastic reduction and viscosity reduction heating unit adopts a heating furnace. The wax oil from the separation unit 6 and / or the wax oil from other processes are added to the heating furnace at the starting end and the end of the front section rough furnace tube through the circulating oil inlet 18, 19. After plastic reduction, viscosity reduction, cracking and heating, high-temperature waste plastic oil is obtained. The high-temperature waste plastic oil enters the pyrolysis reaction unit 5 through pipeline 10 for pyrolysis reaction to obtain pyrolysis products and coke; the pyrolysis products enter the subsequent separation unit 6 through pipeline 11 for separation treatment: the dry gas exits the device from the gas outlet 14, the liquefied gas and gasoline fractions exit the device from the liquefied gas and gasoline fraction outlet 13, and the diesel fraction exits the device from the diesel fraction outlet 12; the wax oil fraction at the bottom of the tower is led out of the separation unit through the wax oil fraction outlet 15, wherein part of the wax oil fraction can also be used as circulating oil to return to the plastic reduction and viscosity reduction heating unit 4 through the circulating oil inlets 18 and 19 for re-refining, and can also be used as a product leading device through pipeline 16.
[0083] The present invention is further described in detail by way of examples. The raw materials used in the examples can be obtained through commercial sources.
[0084] Among them, the analysis method for chlorine content in liquefied waste plastics is: Q / SH 3360 270-2018.
[0085] The analysis methods for other elements in liquefied waste plastics are: carbon and hydrogen elements SH / T 0656-2017, oxygen element SH / T0986, nitrogen element SH / T 0704-2010, and sulfur element SH / T 0842-2010.
[0086] The distribution of pyrolysis products was obtained by simulated distillation NB / SH / T 0829-2010 method.
[0087] The density analysis method of diesel wax oil is SH / T0604-2000; the composition of pyrolysis gas is determined by RIPP 78-90 method; the hydrocarbon composition of naphtha, diesel, etc. is determined by chromatography analysis.
[0088] In the following examples, the particle size of the particles obtained by the pulverization process ranges from 100 to 2000 μm.
[0089] Example 1
[0090] Example 1 illustrates the technical effect of the pyrolysis and cracking processing method of waste plastics provided by the present invention.
[0091] The process flow is as follows Figure 2 As shown, the waste plastic melting and dechlorination unit 2 adopts the second twin-screw heating and conveying equipment, the gas phase outlet of the second twin-screw heating and conveying equipment is connected to the vacuum equipment and the hydrogen chloride absorption unit 7, the waste plastic liquefaction unit adopts the first twin-screw heating and conveying equipment, the plastic reduction and viscosity reduction heating unit adopts a heating furnace, and the second twin-screw heating and conveying equipment, the first twin-screw heating and conveying equipment and the heating furnace are connected in sequence. In the heating furnace, the front section thick furnace tube and the rear section thin furnace tube are directly connected, and the inner diameter ratio of the front section thick furnace tube and the rear section thin furnace tube is 2:1, and the length ratio is 0.4:1.
[0092] The waste agricultural film (mainly made of PE, with a chlorine content of 0.0162% by weight) is heated and melted in the second twin-screw heating and conveying equipment, with a feed rate of about 100 kg / h, an outlet temperature of 220°C, and a processing time of 6 minutes. During the hot-melt dechlorination process, a vacuum system is used to extract the gas phase material containing hydrogen chloride and send it to the hydrogen chloride absorption unit, where it contacts the hydrogen chloride absorbent (NaOH solution) for hydrogen chloride absorption treatment. The vacuum degree of the second twin-screw heating and conveying equipment is 150 mmHg. After hot-melt dechlorination treatment, the dechlorinated waste plastic WP-1 is obtained, and the properties are shown in Table 1.
[0093] After dechlorination, the waste plastic WP-1 enters the first twin-screw heating and conveying equipment for liquefaction treatment to obtain liquefied waste plastic. The outlet temperature of the liquefied waste plastic of the first screw heating and conveying equipment is 360℃, and the residence time is 6min. The liquefied waste plastic at the outlet of the first twin-screw heating and conveying equipment enters the heating furnace, and the reaction temperature in the front thick furnace tube is 360℃~380℃, and the residence time is 30min. The material continues to heat up rapidly from 380℃ to 500℃ in the rear thin furnace tube to obtain high-temperature liquefied waste plastic oil. The gas injection volume is 0, and the outlet temperature of the heating furnace is 500℃. The high-temperature liquefied waste plastic oil enters the pyrolysis tower and undergoes pyrolysis reaction under the conditions of 0.2MPa and 500℃. The operation cycle is 2h to obtain pyrolysis products and coke. The obtained pyrolysis products enter the separation unit for separation to obtain dry gas, liquefied gas, gasoline fraction, diesel fraction and wax oil fraction, and the product distribution test is carried out. The distribution of pyrolysis reaction products is shown in Table 2 and Table 3.
[0094] As can be seen from Example 1, the dechlorinated waste plastic WP-1 is obtained after the waste agricultural film is melted and liquefied by a twin-screw heating and conveying equipment through a dechlorination process. Since most of the chlorine in the waste agricultural film is inorganic chlorine, it is not decomposed into hydrogen chloride during the dechlorination process, but enters into the treated waste plastic. Therefore, the chlorine content of WP-1 remains unchanged.
[0095] Example 2
[0096] The process flow is the same as that of Example 1, and the waste plastic (mainly made of PE and PU) is placed in the second twin-screw heating and conveying device for melting and dechlorination to obtain the dechlorinated waste plastic WP-2, and the properties are shown in Table 1. The feed rate of the second twin-screw heating and conveying device is about 100 kg / h, the outlet temperature is 300° C., the processing time is 5 min, the vacuum degree of the second twin-screw heating and conveying device is 70 mmHg, and the absorption process of the hydrogen chloride-containing gas obtained by the dechlorination treatment is the same as that of Example 1.
[0097] After dechlorination, the waste plastic WP-2 enters the first twin-screw heating and conveying equipment for liquefaction treatment to obtain liquefied waste plastic. The outlet temperature of the first twin-screw heating and conveying equipment is 360° C., and the residence time is 0.1 h.
[0098] The liquefied waste plastic enters the heating furnace, and the front thick furnace tube and the rear thin furnace tube of the heating furnace are directly connected. The inner diameter ratio of the front thick furnace tube and the rear thin furnace tube is 3:1, and the length ratio is 0.3:1. The reaction temperature of the front thick furnace tube is 360℃-400℃, and the residence time is 30min. The rear thin furnace tube continues to rapidly heat up from 400℃ to 480℃ to obtain high-temperature liquefied waste plastic oil.
[0099] The high-temperature liquefied waste plastic oil enters the pyrolysis tower for pyrolysis reaction. The top pressure of the pyrolysis tower is 0.2MPa, the pyrolysis reaction temperature is 480°C, the operation cycle is 5h, and pyrolysis products and coke are obtained.
[0100] The obtained pyrolysis products were separated into dry gas, liquefied gas, gasoline fraction, diesel fraction and wax oil fraction by a separation unit, and the product distribution test was carried out. The distribution of pyrolysis reaction products is shown in Tables 2 and 3.
[0101] It can be seen from Table 2 that since the waste plastic contains a certain amount of polyester and the raw materials contain a certain amount of oxygen after long-term oxidation, the pyrolysis products contain a certain amount of CO2.
[0102] Example 3
[0103] The waste plastic continuous pyrolysis device comprises a first twin-screw heating and conveying device, a heating furnace, a pyrolysis tower and a fractionation tower connected in sequence; the furnace tube of the heating furnace is composed of a front thick furnace tube and a rear thin furnace tube.
[0104] The dechlorinated waste plastic WP-1 in Example 1 was used as a raw material and liquefied by a first twin-screw heating and conveying device to obtain liquefied waste plastic. The feed rate of the first twin-screw heating and conveying device was about 5 kg / h, the outlet temperature of the liquefied waste plastic was 340°C, and the residence time was 12 min.
[0105] The liquefied waste plastic then enters the heating furnace for viscous cracking treatment. The inner diameter ratio of the front thick furnace tube and the rear thin furnace tube of the heating furnace is 4:1, and the length ratio is 0.2:1. The reaction temperature of the front thick furnace tube is 340℃-400℃, the residence time is 50min, and the outlet temperature of the rear thin furnace tube is 520℃.
[0106] The obtained high-temperature liquefied waste plastic oil enters the pyrolysis tower. When the top pressure of the pyrolysis tower is 0.15 MPa, the pyrolysis reaction temperature is 520°C, the operation cycle is 10 hours, the distribution of pyrolysis products is shown in Table 4, the distribution of gas phase products is shown in Table 5, and the liquid products are cut to obtain gasoline, diesel and wax oil components, whose properties are shown in Table 6, and the properties of the coke products are shown in Table 7.
[0107] As can be seen from Example 3, after the waste agricultural film is pyrolyzed and cracked by the method provided by the present invention, the pyrolysis liquid yield (including liquefied gas) can reach 85.84%. The obtained gasoline, diesel and wax oil have a high mass fraction of hydrogen, a high mass fraction of olefins, a low mass fraction of aromatics, and a low content of chlorine and silicon heteroatoms, and can be directly sent to the refinery for post-processing. The sum of the mass fractions of ethylene, propylene and butene in the pyrolysis gas is high (>45% by weight), and the ash content of the coke is as high as 50.5% by weight, which cannot be sold as a product, but can be used as a boiler fuel for blending.
[0108] Comparative Example 1
[0109] The same waste plastic raw material as in Example 3 was used, except that the waste plastic raw material was not subjected to liquefaction treatment and plastic reduction and viscosity reduction treatment, but was directly introduced into an autoclave, the reaction temperature was set to 500°C, and the residence time was 2h. A pyrolysis reaction was performed to obtain pyrolysis products and coke, and the pyrolysis products were separated into dry gas, liquefied gas, gasoline fraction, diesel fraction, and wax oil fraction by entering a separation unit. The conditions were the same as in Example 3. The product distribution is shown in Table 5.
[0110] It can be seen from Comparative Example 1 that the same raw materials as those in Example 3 cannot be pumped to achieve high-density continuous feeding due to the lack of liquefaction and plastic reduction treatment. The batch reaction processing capacity is small when using a kettle reactor. In addition, solid plastic is a poor conductor of heat, so the heat transfer is slow and uneven, which can easily cause the problem of local excessive cracking. Therefore, compared with Example 3, the yields of dry gas and liquefied gas, gasoline and coke in Comparative Example 1 are increased, the yields of diesel and wax oil are decreased, and the total liquid yield is also decreased.
[0111] Comparative Example 2
[0112] The waste plastic continuous pyrolysis device comprises a first twin-screw heating and conveying device, an adiabatic upflow viscosity-reducing reactor, a heating furnace, a pyrolysis tower and a fractionation tower which are connected in sequence.
[0113] The dechlorinated waste plastic WP-1 in Example 1 is used as a raw material, and the first twin-screw heating and conveying equipment is used for liquefaction treatment to obtain liquefied waste plastic. The feed rate of the first twin-screw heating and conveying equipment is about 5kg / h, the outlet temperature of the liquefied waste plastic is 380°C, and the residence time is 6min. Then, the visbreaking treatment is carried out in an adiabatic upflow visbreaking reactor, the visbreaking temperature is 380°C, and the visbreaking time is 1h. The visbreaking material enters the heating furnace for heating and heating, and the outlet temperature of the heating furnace is 520°C. The high-temperature waste plastic oil from the heating furnace enters the pyrolysis tower for pyrolysis reaction to obtain pyrolysis products and coke; the pyrolysis products enter the fractionation tower for separation, and when the pressure of the pyrolysis tower is 0.15MPa, the reaction temperature of the pyrolysis tower is 520°C, the operation cycle is 6h, and the distribution of pyrolysis products is shown in Table 4.
[0114] It can be seen from Comparative Example 2 that the raw materials are the same as those in Example 3, and the difference in the process is that the heating furnace tube in Comparative Example 2 has no variable diameter design. Since the plastic reduction and viscosity reduction reaction time is longer than that in Example 3, the yields of dry gas, liquefied gas and coke are slightly higher than those in Example 3, but its process flow is longer than that in Example 3, and more equipment is required.
[0115] Example 4
[0116] Example 4 illustrates the technical effect of the waste plastic melting and dechlorination unit in step S0 of the present invention.
[0117] The waste plastic melting dechlorination unit includes a second screw heating and conveying device and a vacuum device connected to the second screw heating and conveying device. The second screw heating and conveying device adopts a twin-screw heating and conveying device. During the dechlorination process, a vacuum system is used to extract the gas phase material containing hydrogen chloride and send it to the hydrogen chloride absorption unit, and contact with the hydrogen chloride absorbent (NaOH solution) for hydrogen chloride absorption treatment. Waste plastics (made of PE, PP, PS, PVC, etc., with a chlorine content of about 9% by weight) enter the second screw heating and conveying device for hot melt dechlorination treatment to obtain dry gas containing hydrogen chloride and dechlorinated waste plastic materials. The feeding rate of the twin-screw heating and conveying equipment is about 100kg / h. Different outlet temperatures are set at 260℃, 300℃, 320℃, and 360℃. The reaction time is 0.1h. The vacuum degree of the vacuum device is 150mmHg. Waste plastic samples WP-4-260, WP-4-300, WP-4-320, and WP-4-360 are obtained respectively, and their properties are shown in Table 8.
[0118] It can be seen from Example 4 that as the outlet temperature of the second heating and conveying dechlorination screw increases, the chlorine content in the waste plastics continues to decrease. When the outlet temperature is greater than 300° C., the dechlorination rate is relatively high.
[0119] Table 1 Properties of waste plastics after dechlorination
[0120] Example 1 Example 2 Sample name WP-1 WP-2 Average particle size, μm 1500 1800 Ash / wt% 2.86 11.58 w(C) / % 83.28 65.47 w(H) / % 13.25 9.59 w(S) / % <0.1 0.16 w(N) / % 0.028 0.05 w(Cl) / % 0.0162 0.39 w(Si) / % 0.131 2.07 w(O) / % 1.45 7.17 w(Ca)% 0.709 w(Al)% 5.51
[0121] Table 2 Distribution of pyrolysis products of waste plastics
[0122]
[0123]
[0124] Table 3 Mass composition of dry gas and liquefied gas produced by pyrolysis of waste plastics
[0125] Example Example 1 Example 2 Composition / weight% Dry gas 46.90 46.02 hydrogen 1.80 0.24 Methane 7.47 7.49 Ethane 21.51 19.82 Ethylene 16.11 18.48 Liquefied gas 53.10 53.98 Propylene 21.03 20.67 Butene 12.27 15.11 Propane 14.18 13.28 Isobutane 0.13 0.14 n-Butane 5.49 5.81 total 100.00 100.00
[0126] Table 4 Distribution of pyrolysis products of waste plastics
[0127]
[0128] Table 5 Composition of waste plastic pyrolysis gas
[0129]
[0130]
[0131] Table 6 Properties of liquid products in the pyrolysis products of waste plastics
[0132]
[0133]
[0134] Table 7 Properties of coke in waste plastic pyrolysis products
[0135]
[0136]
[0137] Table 8 Properties of dechlorinated waste plastics under different temperature conditions in Example 4
[0138]
[0139] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0140] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the content of the present invention.
Claims
1. A method for pre-treating waste plastics by pyrolysis and cracking, It is characterized in that include: S1, the waste plastics to be processed enter the waste plastics liquefaction unit for liquefaction treatment to obtain liquefied waste plastics, and the waste plastics liquefaction unit adopts a screw-type heating and conveying equipment; S2. The liquefied waste plastic enters the plastic reduction and viscosity reduction heating unit for plastic reduction and viscosity reduction cracking treatment to obtain high-temperature liquefied waste plastic oil and dry gas after plastic reduction and viscosity reduction cracking; the plastic reduction and viscosity reduction heating unit adopts a heating furnace, and its heating furnace tube consists of a front section thick furnace tube and a rear section thin furnace tube.
2. The method for pretreatment of waste plastics by pyrolysis and cracking according to claim 1, It is characterized in that The operating conditions of the liquefaction treatment in S1 are: the outlet temperature of the liquefied waste plastic is 330-380° C., preferably 340-360° C.; the residence time is 1-20 min, preferably 5-15 min.
3. The method for pretreatment of waste plastics by pyrolysis and cracking according to claim 1 or 2, It is characterized in that The inner diameter ratio of the front thick furnace tube and the rear thin furnace tube is 2-4:1, preferably 2-3:1; the length ratio of the front thick furnace tube and the rear thin furnace tube is 0.1-0.6:1, preferably 0.2-0.6:
1.
4. The method for pretreatment of waste plastics by pyrolysis and cracking according to claim 3, It is characterized in that The operating conditions of the rough furnace tube in the front section of the heating furnace in S2 are: reaction temperature is 360-420°C, preferably 380-400°C; residence time is 10-60 min, preferably 15-30 min.
5. The method for pretreatment of waste plastics by pyrolysis and cracking according to claim 3, It is characterized in that The operating conditions of the thin furnace tubes in the rear section of the heating furnace in S2 are: the outlet temperature of the heating furnace is 480°C to 550°C, preferably 480°C to 540°C; the steam injection amount is 0 to 5% by weight, preferably 0.5 to 3% by weight.
6. A waste plastic pyrolysis cracking pretreatment reaction device, comprising a first screw-type heating and conveying device and a heating furnace directly connected thereto, wherein the furnace tube of the heating furnace is composed of a front-stage thick furnace tube and a rear-stage thin furnace tube connected; in, The inner diameter ratio of the front thick furnace tube and the rear thin furnace tube is 2-4:1, preferably 2-3:1; the length ratio of the front thick furnace tube and the rear thin furnace tube is 0.1-0.6:1, preferably 0.2-0.6:
1.
7. A method for pyrolysis and cracking of waste plastics, It is characterized in that A pretreatment method for pyrolysis and cracking of waste plastics comprising any one of claims 1 to 5, and, S3, the high temperature liquefied waste plastic oil enters the pyrolysis reaction unit for pyrolysis reaction to obtain pyrolysis products and coke; S4. The pyrolysis products enter a separation unit for separation to obtain dry gas, liquefied gas, gasoline fraction, diesel fraction and wax oil fraction.
8. The method for pyrolysis and cracking of waste plastics according to claim 7, It is characterized in that In step S3, the operating conditions of the pyrolysis reaction include: the top pressure of the pyrolysis tower is 0.05-0.6 MPa, preferably 0.1-0.3 MPa; the pyrolysis reaction temperature is 450-580°C, preferably 480-550°C, and the pyrolysis tower operation cycle is 1h-500h, preferably 10h-240h.
9. The method for pyrolysis and cracking of waste plastics according to claim 7 or 8, It is characterized in that The wax oil fraction is returned to step S2 for recycling, the recycled wax oil fraction is added to the starting end of the front thick furnace tube, and the weight ratio of the recycled wax oil fraction to the liquefied waste plastic is 0.2 to 5.0:1, preferably 0.2 to 2:1; Preferably, the wax oil fraction is a fraction with a distillation range of more than 350° C. obtained by separation of the separation unit or a fraction with a distillation range of more than 350° C. obtained by other processes.
10. The method for pyrolysis and cracking of waste plastics according to claim 7 or 8, It is characterized in that Also includes: S0, the chlorine-containing waste plastic raw material enters the waste plastic melting dechlorination unit for hot melt dechlorination treatment to obtain dry gas containing hydrogen chloride and dechlorinated waste plastic material; the dechlorinated waste plastic material directly enters the waste plastic liquefaction unit of S1; or the dechlorinated waste plastic material is cooled and crushed in turn to obtain dechlorinated waste plastic particles, and the dechlorinated waste plastic particles enter the waste plastic liquefaction unit of S1.
11. The method for pyrolysis and cracking of waste plastics according to claim 10, It is characterized in that The waste plastic melting dechlorination unit comprises a second screw-type heating and conveying device and a vacuum device connected to the second screw-type heating and conveying device; Preferably, the second screw heating and conveying equipment is selected from a twin-screw or single-screw conveying equipment; the process conditions of the melt dechlorination treatment include: a feed rate of 5 to 5000 kg / h, preferably 100 to 4000 kg / h; an outlet temperature of 150 to 370°C, preferably 300 to 330°C, a reaction time of 0.1 to 0.5h, preferably 0.1 to 0.3h; the vacuum degree of the waste plastic melt dechlorination unit is 50 to 300 mmHg, preferably 50 to 150 mmHg; preferably, the particle size of the dechlorinated plastic particles obtained by pulverization treatment is 100 to 2000 μm.
12. The method for pyrolysis and cracking of waste plastics according to claim 10 or 11, It is characterized in that Step S0 also includes: allowing the obtained dry gas containing hydrogen chloride to enter a hydrogen chloride absorption unit, contacting with a hydrogen chloride absorbent to perform hydrogen chloride absorption treatment, and obtaining a chlorine-containing absorbent and a dechlorinated dry gas; optionally, allowing the dry gas containing hydrogen chloride to enter the hydrogen chloride absorption unit under the action of a vacuum system; wherein the hydrogen chloride absorbent is water or an alkali solution with a pH greater than 7; optionally, the alkali solution includes one or more of a sodium hydroxide solution, a potassium hydroxide solution, a calcium hydroxide solution, a sodium bicarbonate solution, a sodium carbonate solution and an ammonia solution.
13. The method for pyrolysis and cracking of waste plastics according to claim 7, It is characterized in that The waste plastics to be processed include one or more of LDPE, HDPE, PS, PP, PET and PVC; optionally, the content of PVC in the waste plastics to be processed is less than 10 weight %; the ash content in the waste plastics to be processed is 1 to 40 weight %, preferably 3 to 30 weight %.
14. A waste plastic pyrolysis and cracking processing system, It is characterized in that The invention comprises a first twin-screw heating and conveying device, a heating furnace, a pyrolysis tower and a fractionation tower which are connected in sequence; the furnace pipe of the heating furnace is composed of a front thick furnace pipe and a rear thin furnace pipe.
15. The waste plastic pyrolysis and cracking processing system according to claim 14, It is characterized in that The inner diameter ratio of the front thick furnace tube and the rear thin furnace tube is 2-4:1, preferably 2-3:1; the length ratio of the front thick furnace tube and the rear thin furnace tube is 0.1-0.6:1, preferably 0.2-0.6:
1.
16. The waste plastic pyrolysis and cracking processing system according to claim 14 or 15, It is characterized in that It also includes a second screw heating and conveying device and a vacuum device, wherein the gas phase outlet of the second screw heating and conveying device is connected to the vacuum device, and the material outlet of the second screw heating and conveying device is connected to the material inlet of the first twin-screw heating device.
Citation Information
Patent Citations
Coking method for producing fuel oil from waste plastics
CN104611030A
Waste plastic continuous thermal cracking system and cracking method thereof
CN109401774A
Method and apparatus for co-converting waste plastic in delayed coker unit
CN112538363A
Steam cracking method
CN106635125A
Method and system for recycling waste plastics through pyrolysis
CN116064064A
Cited By
Waste plastic pyrolysis unit
TWI927623B