Preparation method of sintered ore
By mixing and granulation multiple times to form a high-alkaline adhesion layer, and feeding oxygen at the stage during the sintering process, the problem of low mineralization efficiency in sintering of high proportion concentrate is solved, and the yield rate and drum strength of the sintered ore are improved. .
Patent Information
- Application Number
- CN202411246757.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art lacks attention to high-temperature mineralization processes during the sintering of high proportion concentrates, resulting in low mineralization efficiency and yield.
A sintered ore preparation method is adopted, by mixing iron ore, flux, active calcium and iron additives and fuel multiple times to form a high alkaline adhesion layer, and the sintered material surface is divided into multiple In the area, different oxygen concentrations are set to strengthen the oreing reaction.
The ore formation rate and yield of the sintered ore are improved, the drum strength is enhanced, and the molar ratio of CaO/Fe2O3 is more suitable, which improves the overall performance of the sintered ore.
Smart Images

Figure CN119061260A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of sintering process of iron and steel metallurgy, and in particular to a method for preparing sintered ore. Background Art
[0002] Sintered ore is the main iron-containing charge for blast furnace ironmaking, and its proportion in domestic steel enterprises exceeds 70%. There are many types of sintering raw materials, including fine-grained iron concentrate, coarse-grained iron ore powder, flux, fuel, return ore, etc. Most steel companies also add iron-containing dust and mud for internal consumption in the sintering process. Therefore, the physical and chemical properties of sintered materials will have an important impact on the subsequent granulation and sintering links, and even the steel smelting process.
[0003] In recent years, more and more fine-grained iron ore has poured into the international iron ore market, causing many domestic and foreign steel companies to add more fine-grained materials to organize sintering production. At present, the domestic strengthening of high-proportion concentrate sintering is mainly focused on strengthening raw material mixing and granulation. For example, the use of strong mixing to improve the mixing and subsequent granulation process can reduce the powder loss rate of the mixed material after granulation and improve the air permeability of the sintering material layer; the use of composite binders also has a good strengthening effect on the mixing and granulation of sintering raw materials, and can improve the utilization factor of the sintering machine. The above methods focus on strengthening the mixing of raw materials to strengthen the subsequent sintering process, but lack attention to the high-temperature mineralization process of the sintering process. Summary of the invention
[0004] The present application provides a method for preparing sintered ore to solve the following technical problem: providing a new method for preparing sintered ore.
[0005] In a first aspect, the present application provides a method for preparing sintered ore, the method comprising:
[0006] Obtaining raw materials, the raw materials include iron ore, flux, active calcium iron additive, return ore and fuel, wherein the iron ore includes fine-grained iron-containing material, the fine-grained iron-containing material includes a first fine-grained iron-containing material and a second fine-grained iron-containing material, the flux includes a first flux and a second flux, and the active calcium iron additive includes a first active calcium iron additive and a second active calcium iron additive;
[0007] The first fine iron-containing material, the second active calcium iron additive, the first flux, the return ore and the fuel are first mixed and first granulated to obtain first mixed material balls;
[0008] The first mixed material ball, the second fine iron-containing material, the second active calcium iron additive and the second flux are subjected to second mixing and second granulation to obtain a second mixed material ball having a high alkalinity adhesion layer;
[0009] The second mixed material balls are sintered, and the sintered material surface is divided into a plurality of regions, and the oxygen concentration of each region is set to obtain sintered ore.
[0010] Optionally, the weight ratio of the first fine-grained iron-containing material to the second fine-grained iron-containing material is (90-95):(5-10).
[0011] Optionally, the weight ratio of the first active calcium iron additive to the second active calcium iron additive is (70-80):(20-30).
[0012] Optionally, the weight ratio of the first flux to the second flux is (70-80):(20-30).
[0013] Optionally, the fine-grained iron-containing material is 0.8 parts by weight or more relative to 1 part by weight of the iron ore.
[0014] Optionally, in terms of mass fraction, the content of the iron ore is 55% to 70%, the content of the flux is 10% to 15%, the content of the active calcium iron additive is 0.3% to 1%, the content of the returned ore is 15% to 25%, and the content of the fuel is 3% to 5%.
[0015] Optionally, the fine-grained iron-containing material includes fine-grained iron concentrate, gas ash and converter mud; wherein, by mass fraction, the content of fine-grained iron concentrate is 90% to 100%, the content of gas ash is 0 to 10%, and the content of converter mud is 0 to 10%.
[0016] Optionally, the active calcium iron additive includes at least one of the following: limestone, dolomite, calcium ferrite; and / or,
[0017] The flux includes at least one of the following: quicklime, limestone, and dolomite.
[0018] Optionally, sintering the second mixed material ball, dividing the sintered material surface into a plurality of regions, and setting the oxygen concentration of each region to obtain the sintered ore includes:
[0019] Sintering the second mixed material ball, dividing the sintered material surface into at least three areas, and setting the oxygen concentration of each area to obtain sintered ore; wherein the at least three areas include: a first area, a second area and a third area;
[0020] The area of the first region is 40% to 45%, the area of the second region is 30% to 35%, and the area of the third region is 20% to 30%.
[0021] Optionally, the oxygen volume fraction in the first region is 22.0% to 23.0%, the oxygen volume fraction in the second region is 21.0% to 22.0%, and the oxygen volume fraction in the third region is 20.5% to 21.0%.
[0022] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0023] The preparation method of the sintered ore provided in the embodiment of the present application includes: obtaining raw materials, the raw materials including iron ore, flux, active calcium iron additive, return ore and fuel, wherein the iron ore includes fine-grained iron-containing material, the fine-grained iron-containing material includes a first fine-grained iron-containing material and a second fine-grained iron-containing material, the flux includes a first flux and a second flux, and the active calcium iron additive includes a first active calcium iron additive and a second active calcium iron additive; performing a first mixing and a first granulation on the first fine-grained iron-containing material, the second active calcium iron additive, the first flux, the return ore and the fuel to obtain a first mixed ball; performing a second mixing and a second granulation on the first mixed ball, the second fine-grained iron-containing material, the second active calcium iron additive and the second flux to obtain a second mixed ball with a high alkalinity adhesion layer; sintering the second mixed ball, dividing the sintered sintering material surface into a plurality of areas, and setting the oxygen concentration of each of the areas to obtain a sintered ore. The first mixed material ball provides a basis for the subsequent adhesion of the high alkalinity adhesion layer on the surface of the first mixed material ball. The second fine iron-containing material participates in the second granulation process as an adhesion powder in the preparation of the second mixed material ball, which helps the adhesion and growth of the second mixed material ball; the second active calcium iron additive and the second flux help to regulate the alkalinity of the adhesion layer of the second mixed material ball in the preparation of the second mixed material ball, form a high alkalinity adhesion layer, and strengthen the subsequent mineralization process; the second mixed material ball is sintered, and different oxygen concentrations are provided on the sintering material surface to increase the oxygen potential of the magnetite concentrate oxidation in the second mixed material ball, promote its conversion to hematite, and thus strengthen the mineralization reaction between it and the calcium flux. In summary, the high-alkalinity adhesion layer strengthens the mineralization process and the step-by-step oxygen-enriched sintering strengthens the oxidation process, strengthens the high-proportion concentrate sintering process, increases the amount of calcium ferrite generated in the sintered ore mineralization process, and makes the CaO / Fe2O3 molar ratio in the mineralization process tend to an appropriate level (0.6-0.8), and improves the sintered ore yield and drum strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0026] Figure 1 A schematic flow chart of a method for preparing sintered ore provided in an embodiment of the present application. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0028] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0029] In this application, the terms "include", "comprises", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0031] In a first aspect, the present application provides a method for preparing sintered ore. Figure 1 For a schematic diagram of a method for preparing sintered ore provided in an embodiment of the present application, see Figure 1 , the method comprising:
[0032] S1. obtaining raw materials, the raw materials comprising iron ore, flux, active calcium iron additive, return ore and fuel, wherein the iron ore comprises fine-grained iron-containing material (the content of -200 mesh in the material accounts for more than 50%), the fine-grained iron-containing material comprises a first fine-grained iron-containing material and a second fine-grained iron-containing material, the flux comprises a first flux and a second flux, and the active calcium iron additive comprises a first active calcium iron additive and a second active calcium iron additive;
[0033] S2, performing a first mixing and a first granulation on the first fine-grained iron-containing material, the second active calcium iron additive, the first flux, the return ore and the fuel to obtain a first mixed material ball;
[0034] S3, performing a second mixing and second granulation on the first mixed material ball, the second fine iron-containing material, the second active calcium iron additive and the second flux to obtain a second mixed material ball having a high alkalinity adhesion layer;
[0035] In the embodiment of the present application, the first mixture ball provides a basis for the subsequent attachment of a high alkalinity adhesion layer on the surface of the first mixture ball. The second fine-grained iron-containing material participates in the second granulation process as an adhesion powder in the preparation of the second mixture ball, which helps the adhesion and growth of the second mixture ball. The second active calcium iron additive and the second flux help to regulate the alkalinity of the adhesion layer of the mixture ball in the preparation of the second mixture ball, form a high alkalinity adhesion layer, and enhance the subsequent mineralization process.
[0036] In some embodiments, the weight ratio of the first fine iron-containing material to the second fine iron-containing material is (90-95):(5-10).
[0037] In the embodiment of the present application, a high proportion of the iron-containing material added in the first stage can ensure the granulation effect, and the proportion of the iron-containing material added in the second stage is controlled to be low because the formation of the high alkalinity adhesion layer is controlled in the outer layer of the pellets, and there is no need for too much proportion of fine iron-containing material. Exemplarily, the weight ratio of the first fine iron-containing material to the second fine iron-containing material can be 90:10, 95:5, 91:9, 92:8, 93:7, 94:6, etc.
[0038] In some embodiments, the weight ratio of the first active calcium iron additive to the second active calcium iron additive is (70-80):(20-30).
[0039] In the embodiment of the present application, the weight ratio of the first active calcium iron additive to the second active calcium iron additive is limited, in order to form a strengthened mineralization adhesion layer in the second stage, which is conducive to the formation of a calcium ferrite liquid phase in the subsequent mineralization process. Exemplarily, the weight ratio of the first active calcium iron additive to the second active calcium iron additive can be 70:30, 75:25, 80:20, 78:22, 73:27, etc.
[0040] In some embodiments, the weight ratio of the first flux to the second flux is (70-80):(20-30).
[0041] In the embodiment of the present application, the weight ratio of the first flux to the second flux is limited. In order to ensure the high alkalinity of the adhesion layer, the reaction conditions of high alkalinity are conducive to the formation of the calcium ferrite liquid phase in the subsequent mineralization process. Exemplarily, the weight ratio of the first flux to the second flux can be 70:30, 75:25, 80:20, 78:22, 73:27, etc.
[0042] In some embodiments, the fine iron-containing material is 0.8 parts by weight or more relative to 1 part by weight of the iron ore.
[0043] In some embodiments, by mass fraction, the content of the iron ore is 55% to 70%, the content of the flux is 10% to 15%, the content of the active calcium iron additive is 0.3% to 1%, the content of the return ore is 15% to 25%, and the content of the fuel is 3% to 5%.
[0044] In the embodiment of the present application, the amount of the above-mentioned fine iron-containing material, as well as the content of iron ore, flux, active calcium iron additive, return ore and fuel are limited to ensure a high proportion of fine iron-containing material, and to ensure that there is enough flux to form a high alkalinity mineralization environment for the adhesion layer, which is conducive to the formation and mass transfer of the calcium ferrite leading liquid phase in the sintering process. For example, relative to 1 part by weight of iron ore, the fine iron-containing material can be 0.8 parts by weight, 0.85 parts by weight, 0.9 parts by weight, etc. The content of iron ore can be 55%, 58%, 60%, 65%, 70%, the content of the above-mentioned flux is 10%, 11%, 12%, 13%, 14%, 15%, the content of the above-mentioned active calcium iron additive is 0.3%, 0.5%, 0.7%, 0.8%, 1%, the content of the above-mentioned return ore is 15%, 17%, 19%, 22%, 25%, etc., and the content of the above-mentioned fuel is 3%, 4%, 5%, etc. The above iron ore also includes coarse-grained iron ore, which is added in the first mixing.
[0045] In some embodiments, the fine-grained iron-containing material includes fine-grained iron concentrate, gas ash and converter mud; wherein, by mass fraction, the content of fine-grained iron concentrate is 90% to 100%, the content of gas ash is 0 to 10%, and the content of converter mud is 0 to 10%.
[0047] In the embodiment of the present application, fine-grained iron ore is matched with large-grained powder ore to adjust the particle size of sintering raw materials, and the sintering of fine-grained concentrate can achieve effective resource utilization. The gas ash has a high content of Ca and Si, which can adjust the basicity of sintering raw materials, and the burn-off loss is large, which is conducive to the formation of loose and porous sintered ore, and the cost of gas ash is low. The addition of gas ash can effectively utilize resources and reduce sintering costs. Converter mud uses hot gas ash and converter dust mud for sintering production, which can improve the quality of sintered ore, increase its mechanical strength, save fuel, and improve the environment, with significant benefits. The amount of the above-mentioned fine-grained iron ore, gas ash and converter mud is limited, the proportion of fine-grained iron ore is maintained at a high level, and the basicity of raw materials is appropriately adjusted; if the gas ash content is too high, the content of harmful elements such as S and P in the raw materials may be too high, thereby reducing the blast furnace utilization coefficient; if the converter mud content is too high, the Zn content of the raw materials may be too high, which is not conducive to the sintering process. Fine iron ore concentrate, gas ash and converter mud together constitute a raw material of a high proportion of fine iron-containing materials, and can realize the disposal of solid waste resources such as gas ash and converter mud. Exemplarily, the content of the above-mentioned fine iron ore concentrate can be 90%, 92%, 94%, 96%, 98%, 100%, etc., the content of gas ash can be 10%, 8%, 6%, 4%, 2%, etc., and the content of converter mud can be 10%, 8%, 6%, 4%, 2%, etc.
[0048] In addition, the first period of time is 60-80s, which ensures the uniform mixing effect of the mixture and appropriately saves costs; the first granulation time is 4-5min, which ensures the length of one granulation to ensure the effect of one granulation; the second granulation time is 2.5-3.5min. The secondary granulation makes the mixture balls grow further. During this period, high-activity calcium iron additives and part of iron concentrate are added to ensure the formation of an enhanced mineralization layer in the adhesion layer of the mixture balls.
[0049] In some embodiments, the active calcium iron additive comprises at least one of the following: limestone, dolomite, calcium ferrite; and / or,
[0050] The flux includes at least one of the following: quicklime, limestone, and dolomite.
[0051] In an embodiment of the present application, the calcium iron additive is pre-treated with high activity before being added to the raw materials, and the pre-treatment methods include high-pressure roller milling and ball milling. The above-mentioned active calcium iron additive can be one or more of limestone, dolomite, and calcium ferrite, and the above-mentioned flux can be one or more of quicklime, limestone, and dolomite. Before the above-mentioned mixing process, the quicklime is digested with water during the batching, and the digestion time is 4 to 5 minutes. The quicklime digestion reaction generates slaked lime, which has a large specific surface area and can play a partial bonding role. In the above-mentioned first mixing and second mixing, water is generally required to be added. The water content in the above-mentioned second mixed material ball is 7.5 to 8.5%, which can promote combustion, reduce the sintering temperature, and promote the decomposition reaction of the sintering process.
[0052] S4, sintering the second mixed material balls, dividing the sintered material surface into a plurality of regions, and setting the oxygen concentration of each region to obtain sintered ore.
[0053] In some embodiments, sintering the second mixed material ball, dividing the sintered sintering material surface into a plurality of regions, and setting the oxygen concentration of each of the regions to obtain a sintered ore comprises:
[0054] Sintering the second mixed material ball, dividing the sintered material surface into at least three areas, and setting the oxygen concentration of each area to obtain sintered ore; wherein the at least three areas include: a first area, a second area and a third area;
[0055] The area of the first region is 40% to 45%, the area of the second region is 30% to 35%, and the area of the third region is 20% to 30%.
[0056] In some embodiments, the oxygen volume fraction of the first region is 22.0% to 23.0%, the oxygen volume fraction of the second region is 21.0% to 22.0%, and the oxygen volume fraction of the third region is 20.5% to 21.0%.
[0057] In the embodiment of the present application, the materials are placed on the sintering trolley, ignited at the sintering material surface, and the sintering process is carried out. During the sintering process, the trolley is divided into three areas for step-by-step supply of oxygen. Oxygen is added in steps at different stages of the sintering process to increase the oxygen potential of the magnetite concentrate oxidation in the material layer, promote its conversion into hematite, and thus strengthen the mineralization reaction between it and the calcium flux.
[0058] The sintering material surface is divided into three areas, and the method is as follows: from the starting point of sintering to the end point of sintering, it is divided into three areas in sequence. The area of the first area is limited to strengthen the upper layer mineralization reaction; the area of the second area is limited to strengthen the middle layer mineralization reaction; the area of the third area is limited to strengthen the lower layer mineralization reaction. By limiting the oxygen concentration in the first area, the quality deviation of the upper layer sintered ore is caused, and a better concentration of enriched oxygen is supplied, which can effectively improve the occurrence of mineralization reactions in the middle and upper layer sintering process, promote the formation of calcium ferrite leading liquid phase, and improve the quality of this part of the sintered ore; by limiting the oxygen concentration in the second area, the quality of the middle layer sintered ore is relatively good, and the appropriate enriched oxygen concentration is relatively low. While strengthening the middle layer mineralization reaction, it will not supply more enriched oxygen to increase the production cost; by limiting the oxygen concentration in the third area, the quality of the lower layer sintered ore is better, and appropriately increasing the oxygen concentration to strengthen the lower layer mineralization process is beneficial to improving the quality of the lower layer sintered ore, thereby achieving the function of strengthening the overall sintered ore performance indicators. For example, the area of the first region may be 40%, 41%, 42%, 43%, 44%, 45%, etc., the area of the second region may be 30%, 31%, 32%, 33%, 34%, 35%, and the third region may be 20%, 22%, 24%, 26%, 28%, 30%. The oxygen volume fraction of the first region may be 22.0%, 21.0%, 23.0%, etc., the oxygen volume fraction of the second region may be 21.0%, 21.5%, 22.0%, etc., and the oxygen volume fraction of the third region may be 20.5%, 20.6%, 20.7%, 20.8%, 20.9%, 21.0%, etc.
[0059] In summary, the method for preparing sintered ore provided in the embodiment of the present application focuses on the sintering high-temperature mineralization process, from the perspective of the amount of liquid phase generated by calcium ferrite and the liquid phase conduction velocity, by forming an enhanced mineralization layer in the adhesion layer of the mixed material balls and supplying enriched oxygen in a stepwise manner during the sintering process, thereby strengthening the mineralization process of the sintering process, helping to increase the amount of liquid phase generated in the sintering process, and improving the mineralization rate and product quality of the sintered ore.
[0060] The sintered ore prepared in the examples of the present application meets the following properties: the yield is greater than 78.5%, the drum strength is greater than 77.2%, and the utilization coefficient is greater than 1.30.
[0061] The method for preparing sintered ore provided in the embodiment of the present application has at least the following technical effects:
[0062] By adding pretreated high-activity calcium iron additives and flux and part of fine iron-containing materials in the second-stage granulation process, the basicity of the mixed material ball adhesion layer is regulated to form a high-basicity enhanced mineralization layer, so as to achieve the purpose of regulating the CaO / Fe2O3 molar ratio in the molten zone of the sintered ore and promoting the formation of the calcium ferrite leading liquid phase in the sintering process. Compared with uniformly distributing the flux, the formation of the liquid phase and calcium ferrite in the sintering process of the high-proportion concentrate can be increased;
[0063] By supplying oxygen enrichment in stages during the sintering process, the oxidation of a large amount of magnetite concentrate in the fine-grained iron concentrate in the adhesion layer is accelerated. The magnetite concentrate is oxidized by heat release during the drying, preheating, combustion and cooling processes, and is more likely to participate in the solid phase reaction of the sintering process with the flux, thereby strengthening the connection of the mixed material balls, accelerating the full oxidation and growth process of the mixed material balls, and thus accelerating the entire sintering process, which is helpful to improve the yield rate of sintered ore and the drum strength;
[0064] By adding gas ash, converter mud and other raw materials into fine-grained iron-containing materials and utilizing the high carbon content in the gas ash, harmful elements can be removed in a concentrated manner under the high temperature conditions of the sintering process, thereby achieving efficient disposal of iron-containing dust and mud in the sintering process.
[0065] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0066] The embodiment of the present application provides a method for preparing sintered ore, please refer to the raw material composition shown in Table 1, the granulation process parameters shown in Table 2, and the sintering process parameters shown in Table 3.
[0067] Table 1 Raw material composition
[0068]
[0069]
[0070] Table 2 Granulation process parameters
[0071]
[0072] Table 3 Sintering process parameters
[0073]
[0074]
[0075] Comparative Example 1
[0076] The raw materials and pelletizing process parameters of the sintered ore provided in Comparative Example 1 are shown in Tables 4 and 5 below.
[0077] Table 4 Raw material composition
[0078]
[0079] Table 5 Granulation process parameters
[0080] Serial number Mixing time s Granulation time min Granulation ball moisture Comparative Example 1 75 3 7.47
[0081] Comparative Example 2
[0082] The sintered ore provided in Comparative Example 2 adopts a two-stage granulation process, and the raw materials and granulation process parameters are shown in Tables 6 and 7 below.
[0083] Table 6 Raw material composition
[0084]
[0085]
[0086] Table 7 Granulation process parameters
[0087]
[0088] The properties of the sintered ores obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were tested, and the results are shown in Table 8.
[0089] Table 8 Properties of sintered ore
[0090] Serial number Yield / % Drum strength / % Utilization coefficient Example 1 78.50 77.20 1.30 Example 2 78.97 77.68 1.33 Example 3 79.81 78.86 1.38 Example 4 80.34 79.63 1.41 Comparative Example 1 76.58 75.14 1.15 Comparative Example 2 78.01 76.87 1.23
[0091] As shown in Table 8, the process of adding pretreated high-activity calcium iron additives and flux and part of fine iron-containing materials in the two-stage granulation process can improve the sintered ore yield, increase the drum strength of the finished sintered ore, and improve the utilization coefficient. As shown in Example 1 and Comparative Example 2, step-by-step oxygen enrichment during the sintering process can also increase the yield and quality of the sintered ore. As shown in each embodiment, increasing the proportion of the second active calcium iron additive can adjust the alkalinity of the adhesion layer, form a high-alkalinity enhanced mineralization layer, and improve the sintered ore yield, drum strength and utilization coefficient.
[0092] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing sintered ore, It is characterized in that The method comprises: Obtaining raw materials, the raw materials include iron ore, flux, active calcium iron additive, return ore and fuel, wherein the iron ore includes fine-grained iron-containing material, the fine-grained iron-containing material includes a first fine-grained iron-containing material and a second fine-grained iron-containing material, the flux includes a first flux and a second flux, and the active calcium iron additive includes a first active calcium iron additive and a second active calcium iron additive; The first fine iron-containing material, the second active calcium iron additive, the first flux, the return ore and the fuel are first mixed and first granulated to obtain first mixed material balls; The first mixed material ball, the second fine iron-containing material, the second active calcium iron additive and the second flux are subjected to second mixing and second granulation to obtain a second mixed material ball having a high alkalinity adhesion layer; The second mixed material balls are sintered, and the sintered material surface is divided into a plurality of regions, and the oxygen concentration of each region is set to obtain sintered ore.
2. The method according to claim 1, It is characterized in that The weight ratio of the first fine iron-containing material to the second fine iron-containing material is (90-95):(5-10).
3. The method according to claim 1, It is characterized in that The weight ratio of the first active calcium iron additive to the second active calcium iron additive is (70-80):(20-30).
4. The method according to claim 1, It is characterized in that The weight ratio of the first flux to the second flux is (70-80):(20-30).
5. The method according to claim 1, It is characterized in that The fine iron-containing material is 0.8 parts by weight or more relative to 1 part by weight of the iron ore.
6. The method according to claim 1 or 5, It is characterized in that In terms of mass fraction, the content of the iron ore is 55% to 70%, the content of the flux is 10% to 15%, the content of the active calcium iron additive is 0.3% to 1%, the content of the return ore is 15% to 25%, and the content of the fuel is 3% to 5%.
7. The method according to claim 1, It is characterized in that The fine iron-containing materials include fine iron concentrate, gas ash and converter mud; wherein, by mass fraction, The content of fine iron ore concentrate is 90% to 100%, the content of gas ash is 0 to 10%, and the content of converter mud is 0 to 10%.
8. The method according to claim 1, It is characterized in that The active calcium iron additive comprises at least one of the following: limestone, dolomite, calcium ferrite; and / or, The flux includes at least one of the following: quicklime, limestone, and dolomite.
9. The method according to claim 1, It is characterized in that The step of sintering the second mixed material ball, dividing the sintered material surface into a plurality of regions, and setting the oxygen concentration of each region to obtain a sintered ore comprises: Sintering the second mixed material ball, dividing the sintered material surface into at least three areas, and setting the oxygen concentration of each area to obtain sintered ore; wherein the at least three areas include: a first area, a second area, and a third area; The area of the first region is 40% to 45%, the area of the second region is 30% to 35%, and the area of the third region is 20% to 30%.
10. The method according to claim 9, It is characterized in that The oxygen volume fraction of the first region is 22.0% to 23.0%, the oxygen volume fraction of the second region is 21.0% to 22.0%, and the oxygen volume fraction of the third region is 20.5% to 21.0%.
Citation Information
Cited By
Method for sintering, intensifying, uniformly mixing and granulating high-proportion concentrate
CN122521983A