Al-Mg-Mn-Er-Zr alloy powder and application thereof in preparation of aluminum alloy frame for photovoltaic module

By using Al-Mg-Mn-Er-Zr alloy powder and laser melting technology to prepare the aluminum alloy frame of photovoltaic modules, the problem of existing frames breaking during load is solved, and the effect of high strength and toughness is achieved.

CN119061294AInactive Publication Date: 2024-12-03HUANSHENG NEW ENERGY (JIANGSU) CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411163272.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The aluminum alloy frames of existing photovoltaic modules are prone to break during loading, and lack load-bearing capacity and corrosion resistance characteristics, making it difficult to meet the strength requirements of large photovoltaic modules.

Method used

Using Al-Mg-Mn-Er-Zr alloy powder, high-strength aluminum alloy frames are prepared by laser melt metallization and laser sintering technology, and curing heat treatment is carried out to form a common partial polymerization phase of Zr, Mn, and Mg and Al3Er phase to improve the The strength and toughness of the alloy.

Benefits of technology

The yield strength of the aluminum alloy frame is significantly improved, reaching 480~560MPa, effectively alleviating the problem of frame fracture and improving corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061294A_ABST
    Figure CN119061294A_ABST
Patent Text Reader

Abstract

The invention provides Al-Mg-Mn-Er-Zr alloy powder and application of the Al-Mg-Mn-Er-Zr alloy powder in preparation of an aluminum alloy frame for a photovoltaic module, and relates to the technical field of photovoltaic modules. The alloy powder is composed of 1.5%-4.6% of Mg, 4.2%-6.7% of Mn, 0.4%-2.8% of Er, 0.3%-1.6% of Zr and the balance Al, and Mn, Mg and Zr in the alloy powder are subjected to solid solution in an Al matrix and have the solid solution strengthening effect; meanwhile, Mn, Er and an Al matrix form independent precipitation of an Al6Mn phase or synergistic precipitation of an Al6Mn phase and an Al3Er phase, and a second phase strengthening effect can also be generated; in addition, the Al3Er phase can refine alloy grains so as to improve the strength. Therefore, the aluminum alloy frame prepared from the alloy powder has the technical effects of high strength and high toughness, and the problem that the frame is broken when an existing traditional aluminum alloy frame photovoltaic module is loaded can be effectively relieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photovoltaic modules, and in particular to an Al-Mg-Mn-Er-Zr alloy powder and application thereof in preparing an aluminum alloy frame for a photovoltaic module. Background Art

[0002] Photovoltaic frames are an important part of solar photovoltaic modules and are located in the middle and lower reaches of the photovoltaic industry chain. Since photovoltaic frames need to encapsulate materials such as cells, glass, and backplanes, as well as enhance the strength of modules, facilitate transportation, installation, and protect photovoltaic modules, photovoltaic frame products are required to have strong load-bearing capacity and corrosion resistance.

[0003] At present, with the continuous development of the photovoltaic industry, the cells used are getting bigger and bigger, the size of photovoltaic modules is getting bigger and bigger, and photovoltaic modules are getting heavier. The requirements for the bearing strength of the frame are also increasing. Therefore, an aluminum alloy frame with high bearing capacity and high strength is needed.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide an Al-Mg-Mn-Er-Zr alloy powder and an aluminum alloy frame for a photovoltaic module prepared therefrom. The Al-Mg-Mn-Er-Zr alloy prepared from the alloy powder has the technical effects of high strength and high toughness, and can effectively alleviate the problem of frame breakage of existing traditional aluminum alloy frame photovoltaic modules when under load.

[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0007] The present invention provides an Al-Mg-Mn-Er-Zr alloy powder, which comprises the following components by mass percentage: Mg 1.5-4.6%, Mn 4.2-6.7%, Er 0.4-2.8%, Zr 0.3-1.6%, and the balance is Al.

[0008] Furthermore, the alloy powder comprises the following components in percentage by mass: Mg 2-3%, Mn 5.5-6.5%, Er 0.4-1.2%, Zr 0.3-0.8%, and the balance is Al;

[0009] Preferably, the alloy powder comprises the following components in percentage by mass: Mg 2.74%, Mn 6.01%, Er 0.86%, Zr 0.52%, and the balance is Al.

[0010] The present invention provides an application of the Al-Mg-Mn-Er-Zr alloy powder in preparing an aluminum alloy frame for a photovoltaic module;

[0011] The aluminum alloy frame is a high-strength aluminum alloy frame, and the yield strength of the aluminum alloy frame is 480-560 MPa.

[0012] The present invention provides a method for preparing an aluminum alloy frame for a photovoltaic module, the method comprising:

[0013] The Al-Mg-Mn-Er-Zr alloy powder raw materials are weighed according to the component ratio, mixed to obtain a powder material; the powder material is subjected to laser melting metallization and molding to obtain an intermediate aluminum alloy frame; then laser sintering and curing heat treatment are sequentially performed to obtain an aluminum alloy frame for a photovoltaic module.

[0014] Further, the laser melting metallization comprises:

[0015] S1: According to the model data, the powder material A is laid into a single-layer powder bed using a powder spreader, and then the laser heat source scans the powder bed for melting to metalize the single-layer powder bed;

[0016] S2: Repeat step S1 on the metallized single-layer powder bed until the Al-Mg-Mn-Er-Zr alloy frame is formed.

[0017] Furthermore, in the step S1, the powder material A is laid into a single-layer powder bed with a thickness of 20 to 40 μm, preferably 30 μm.

[0018] Furthermore, in step S1, the laser heat source power of the laser heat source scanning the powder bed includes 250-350W;

[0019] And / or, in step S1, the laser scanning speed of the laser heat source scanning the powder bed is 800-1200 mm / s.

[0020] Furthermore, the laser sintering parameters satisfy at least one of the following:

[0021] Laser power is 250-350W;

[0022] Laser scanning speed is 800~1200mm / s;

[0023] The laser scanning interval is 100 μm;

[0024] The phase angle of laser sintering is 67°;

[0025] The spot diameter of laser sintering is 75 μm.

[0026] Furthermore, the aging temperature of the curing heat treatment includes 100 to 500° C., and the aging treatment time includes 1 to 12 hours;

[0027] Preferably, the aging temperature of the curing heat treatment is 320-350° C., and the aging treatment time is 2 hours.

[0028] The present invention provides an aluminum alloy frame for a photovoltaic module, wherein the aluminum alloy frame is mainly prepared by the above-mentioned preparation method of the aluminum alloy frame.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The Al-Mg-Mn-Er-Zr alloy powder provided by the present invention is composed of Mg1.5-4.6%, Mn4.2-6.7%, Er0.4-2.8%, Zr0.3-1.6% and the balance Al. In the alloy powder, Mn, Mg and Zr are solid-dissolved in the Al matrix to form a common segregated phase of Zr, Mn and Mg, which has a solid solution strengthening effect; at the same time, Mn and Er form a single precipitation of Al6Mn phase with the Al matrix or a coordinated precipitation of Al6Mn and Al3Er phases, which can also produce a second phase strengthening effect; in addition, Er forms an Al3Er phase with the Al matrix, which can refine the alloy grains to improve the strength of the Al-Mg-Mn-Er-Zr alloy; in addition, since the Al6Mn particles grow after heat treatment, the dislocation movement barrier is weakened, the stress concentration is relieved, and the toughness of the alloy is also improved. Therefore, the Al-Mg-Mn-Er-Zr alloy prepared from the Al-Mg-Mn-Er-Zr alloy powder of the present application has the technical effects of high strength and high toughness.

[0031] The Al-Mg-Mn-Er-Zr alloy powder provided by the present invention can be widely used in the preparation process of the aluminum alloy frame of the photovoltaic module.

[0032] The present invention provides a method for preparing an aluminum alloy frame for a photovoltaic module. The method uses a laser melting metallization technology to shape an Al-Mg-Mn-Er-Zr alloy powder raw material into an intermediate aluminum alloy frame, and then sequentially performs laser sintering and curing heat treatment to obtain an aluminum alloy frame for a photovoltaic module. The preparation method of the present application can significantly improve the strength of the frame, and after heat treatment, the yield strength can reach 480-560MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1This is a schematic structural diagram of an aluminum alloy frame for a photovoltaic module provided by the present invention. DETAILED DESCRIPTION

[0035] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] According to one aspect of the present invention, an Al-Mg-Mn-Er-Zr alloy powder comprises the following components in mass percentage: Mg 1.5-4.6%, Mn 4.2-6.7%, Er 0.4-2.8%, Zr 0.3-1.6%, and the balance is Al.

[0037] The Al-Mg-Mn-Er-Zr alloy powder provided by the present invention is composed of Mg1.5-4.6%, Mn4.2-6.7%, Er0.4-2.8%, Zr0.3-1.6% and the balance Al. In the alloy powder, Mn, Mg and Zr are solid-dissolved in the Al matrix to form a common segregated phase of Zr, Mn and Mg, which has a solid solution strengthening effect; at the same time, Mn and Er form a single precipitation of Al6Mn phase with the Al matrix or a coordinated precipitation of Al6Mn and Al3Er phases, which can also produce a second phase strengthening effect; in addition, Er forms an Al3Er phase with the Al matrix, which can refine the alloy grains to improve the strength of the Al-Mg-Mn-Er-Zr alloy; in addition, since the Al6Mn particles grow after heat treatment, the dislocation movement barrier is weakened, the stress concentration is relieved, and the toughness of the alloy is also improved. Therefore, the Al-Mg-Mn-Er-Zr alloy prepared from the Al-Mg-Mn-Er-Zr alloy powder of the present application has the technical effects of high strength and high toughness.

[0038] Typical but non-limiting preferred embodiments of the percentage of Mg are: 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5% and 4.6%; typical but non-limiting preferred embodiments of the percentage of Mn are: 4.2%, 4.5%, 5.0%, 5.2%, 5.5%, 6.0%, 6.2% and 6.7%; typical but non-limiting preferred embodiments of the percentage of Er are: 0.4%, 0.8%, 1.0%, 1.4%, 1.8%, 2.0%, 2.4% and 2.8%; typical but non-limiting preferred embodiments of the percentage of Mn are: 0.3%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4% and 1.6%.

[0039] In a preferred embodiment of the present invention, the alloy powder comprises the following components by mass percentage: Mg 2-3%, Mn 5.5-6.5%, Er 0.4-1.2%, Zr 0.3-0.8%, and the balance is Al;

[0040] Preferably, the alloy powder comprises the following components in percentage by mass: Mg 2.74%, Mn 6.01%, Er 0.86%, Zr 0.52%, and the balance is Al.

[0041] In the present invention, the technical effect of the Al-Mg-Mn-Er-Zr alloy powder of the present invention is further optimized by further adjusting and optimizing the usage ratio of the raw materials of each component.

[0042] According to one aspect of the present invention, a use of the above-mentioned Al-Mg-Mn-Er-Zr alloy powder in preparing an aluminum alloy frame for a photovoltaic module;

[0043] The aluminum alloy frame is a high-strength aluminum alloy frame, and the yield strength of the aluminum alloy frame is 480-560 MPa.

[0044] The Al-Mg-Mn-Er-Zr alloy powder provided by the present invention can be widely used in the preparation process of the aluminum alloy frame of the photovoltaic module.

[0045] According to one aspect of the present invention, a method for preparing an aluminum alloy frame for a photovoltaic module comprises:

[0046] The Al-Mg-Mn-Er-Zr alloy powder raw materials are weighed according to the component ratio, mixed to obtain a powder material; the powder material is subjected to laser melting metallization and molding to obtain an intermediate aluminum alloy frame; then laser sintering and curing heat treatment are sequentially performed to obtain an aluminum alloy frame for a photovoltaic module.

[0047] The present invention provides a method for preparing an aluminum alloy frame for a photovoltaic module. The method comprises mixing Al-Mg-Mn-Er-Zr alloy powder, molding the alloy powder into a metallized aluminum alloy frame of a desired shape by laser melting technology, and then sequentially performing laser sintering and curing heat treatment to obtain an aluminum alloy frame for a photovoltaic module. The preparation method of the present application can significantly improve the strength of the frame, and after heat treatment, the yield strength can reach 480-560 MPa.

[0048] In a preferred embodiment of the present invention, the laser melting metallization comprises:

[0049] S1: According to the model data, the powder material A is laid into a single-layer powder bed using a powder spreader, and then the laser heat source scans the powder bed for melting to metalize the single-layer powder bed;

[0050] S2: Repeat step S1 on the metallized single-layer powder bed until the Al-Mg-Mn-Er-Zr alloy frame is formed.

[0051] Preferably, the laser melting metallization method is as follows: the powder spreader first spreads the powder material A into a single-layer powder bed, and then uses a laser heat source with a power of 250 W and a laser scanning speed of 1000 mm / s to scan and melt the powder bed, then controls the piston to lower the substrate to a position of a powder thickness distance, and then uses the powder feeding system to spread the new metal powder on the previously processed metal layer, and after adjustment, processes to the next layer until the sample is completely formed.

[0052] As a preferred embodiment, the present application adopts laser melting metallization to prepare alloy powder into Al-Mg-Mn-Er-Zr alloy frame. Compared with the traditional method, the laser melting metallization process of the present application has the following advantages: ① high bonding strength between the treatment layer and the substrate, ② minimal deformation of the treated part, ③ good processing flexibility and wide applicability.

[0053] In a preferred embodiment of the present invention, the preparation method of the present application further includes the step of cleaning powder of the intermediate aluminum alloy frame obtained by molding after laser melting metallization.

[0054] The powder cleaning includes: on the one hand, the excess powder on the surface of the sample is made to perform irregular up and down and rotational movements through a vibrating and rotating system; on the other hand, compressed air is synchronously blown into the hollow inner cavity of the sample through a compressed air generator and an air inlet pipe, so that the powder in the hollow inner cavity is discharged into a powder collecting cylinder through an air outlet pipe under the action of compressed air.

[0055] In the above preferred embodiment, the powder material A is laid into a single-layer powder bed with a powder thickness of 20 to 40 μm, preferably 30 μm. Under the above powder thickness conditions, the laser melting metallization treatment effect is better. When the powder thickness is greater than 40 μm, the powder layer is too thick, which will cause defects such as underfusion and pores, affecting the sample forming quality; and when the powder layer is too thin, such as less than 200 μm, the manufacturing efficiency will be reduced.

[0056] In the above preferred embodiment, the laser heat source power of the S1 laser heat source scanning the powder bed is 250-350W, and the laser scanning speed is 800-1200mm / s. The implementations other than the above heat source power and laser scanning speed will reduce the energy input of the material, thereby increasing the porosity, thereby generating defects such as pores, and affecting the mechanical properties of the sample.

[0057] In a preferred embodiment of the present invention, the laser sintering parameters satisfy at least one of the following:

[0058] Laser power is 250-350W;

[0059] Laser scanning speed is 800~1200mm / s;

[0060] The laser scanning interval is 100 μm;

[0061] The phase angle of laser sintering is 67°;

[0062] The spot diameter of laser sintering is 75 μm.

[0063] As a preferred embodiment, the present application uses the above laser sintering parameters to sinter the intermediate aluminum alloy frame, which has a better sintering effect. However, embodiments not within the above laser sintering parameters of the present application, such as: a scanning spacing greater than 100 μm, will affect the sample forming quality, causing hole defects to form during the sample forming process, thereby affecting the subsequent strength of the sample.

[0064] In a preferred embodiment of the present invention, the aging temperature of the curing heat treatment includes 100 to 500° C., and the aging treatment time includes 1 to 12 hours;

[0065] In the above preferred embodiment, the aging temperature of the curing heat treatment is 320-350° C., and the aging treatment time is 2 hours.

[0066] Preferably, the method for preparing the aluminum alloy frame for photovoltaic modules comprises the following steps:

[0067] (A) mixing Al-Mg-Mn-Er-Zr alloy powder raw materials according to component proportions to obtain powder material A;

[0068] The powder material A has a particle size of 20 to 60 μm.

[0069] (B) In combination with 3D printing technology, a laser melting metallization method is used to prepare powder material A into an Al-Mg-Mn-Er-Zr alloy frame of a desired shape, followed by a powder cleaning process to obtain an intermediate aluminum alloy frame;

[0070] (C) The intermediate aluminum alloy frame is laser sintered and then placed in a curing furnace for heat treatment to obtain an aluminum alloy frame for a photovoltaic module.

[0071] According to one aspect of the present invention, an aluminum alloy frame for a photovoltaic module is provided, wherein the aluminum alloy frame is mainly prepared by the above-mentioned method for preparing the aluminum alloy frame.

[0072] The technical solution of the present invention will be further described below in conjunction with embodiments.

[0073] Embodiments 1 to 5

[0074] Figure 1 This is a schematic diagram of the structure of the aluminum alloy frame used for photovoltaic modules in this application.

[0075] in: Figure 1 (a) is the left view of the aluminum alloy frame. Figure 1 (b) is a top view of the aluminum alloy frame.

[0076] A method for preparing an aluminum alloy frame for a photovoltaic module, the method comprising:

[0077] (1) See Figure 1 ,according to Figure 1 The structural schematic diagram of the aluminum alloy frame shown is combined with 3D printing technology to obtain the model data of the aluminum alloy frame;

[0078] (2) Weigh Al-Mg-Mn-Er-Zr alloy powder raw materials according to the component ratio, mix them, and obtain powder material A;

[0079] The composition of the Al-Mg-Mn-Er-Zr alloy powder is shown in Table 1.

[0080] Table 1:

[0081]

[0082] Using the model data of step (1), the powder material A is molded into a metallized aluminum alloy frame of a desired shape using a laser melting metallization method.

[0083] The laser melting metallization method is as follows: the powder spreader first spreads the powder material A into a single-layer powder bed, and then uses a laser heat source with a power of 250W and a laser scanning speed of 1000mm / s to scan and melt the powder bed, then controls the piston to lower the substrate to a position of a powder thickness, and then spreads the new metal powder on the previously processed metal layer through the powder feeding system, and after adjustment, processes to the next layer until the sample is completely formed.

[0084] (3) Then, a powder cleaning process is performed to obtain an intermediate aluminum alloy frame, and the intermediate aluminum alloy frame is laser sintered and then heat treated to obtain an aluminum alloy frame for a photovoltaic module.

[0085] The powder cleaning process includes: on the one hand, the excess powder on the surface of the sample is made to perform irregular up and down and rotational movements through a vibrating and rotating system; on the other hand, compressed air is synchronously blown into the hollow inner cavity of the sample through a compressed air generator and an air inlet pipe, so that the powder in the hollow inner cavity is discharged into a powder collecting cylinder through an air outlet pipe under the action of compressed air.

[0086] The parameters of the laser sintering include: laser power of 250-350W; laser scanning speed of 800-1200mm / s; laser scanning spacing of 100μm; laser sintering phase angle of 67°; and laser sintering spot diameter of 75μm.

[0087] The aging temperature of the heat treatment includes 100 to 500° C., and the aging treatment time includes 1 to 12 hours;

[0088] The heat treatment method comprises:

[0089] 1. Place the sample in a muffle furnace for metal aging and set the required temperature. Close the furnace door to increase the temperature.

[0090] 2. Raise the temperature to the required temperature and keep it warm for different time periods;

[0091] 3. After keeping warm for a certain period of time, turn off the switch, let the sample cool naturally to room temperature, open the furnace door and take out the sample;

[0092] Specifically, in this embodiment, the aging temperatures used are 100°C, 200°C, 300°C, 325°C, 350°C, 375°C, 400°C, and 500°C, and the aging time is fixed at 2h; then the aging temperatures are selected to be 325°C and 350°C, and the aging treatment time is 1h, 2h, 3h, 4h, 5h, 6h, 8h, 10h, and 12h.

[0093] Embodiments 6 to 9

[0094] Examples 6 to 9 are the same as Example 1 except that the parameters of the laser sintering in step (3) are different from those in Example 1.

[0095] The parameters of the laser sintering in step (3) are shown in Table 2.

[0096] Table 2:

[0097]

[0098] Note: “-” in the above table means “same as Example 1”.

[0099] Embodiments 10 to 16

[0100] Examples 10 to 16 are the same as Example 1 except that the parameters of the heat treatment in step (3) are different from those in Example 1.

[0101] The parameters of the heat treatment in step (3) are shown in Table 3.

[0102] Table 3:

[0103]

[0104]

[0105] Note: “-” in the above table means “same as Example 1”.

[0106] Comparative Examples 1 to 4

[0107] Comparative Examples 1 to 4 are the same as Example 1 except that the composition of the Al-Mg-Mn-Er-Zr alloy powder is different from that of Example 1.

[0108] The composition of the Al-Mg-Mn-Er-Zr alloy powder is shown in Table 4.

[0109] Table 4:

[0110]

[0111] Note: Comparative Example 1 differs from Example 1 in that Er is not included; Comparative Example 2 differs from Example 1 in that Er is not included, and an equal amount of Er in Example 1 is replaced by Zr; Comparative Example 3 differs from Example 1 in that Er is not included, and an equal amount of Er in Example 1 is replaced by Mg; Comparative Example 4 differs from Example 1 in that Zr is not included.

[0112] Comparative Examples 5 to 12

[0113] Comparative Examples 5 to 12 are the same as Example 1 except that the composition of the Al-Mg-Mn-Er-Zr alloy powder is different from that of Example 1.

[0114] The composition of the Al-Mg-Mn-Er-Zr alloy powder is shown in Table 5.

[0115] Table 5:

[0116]

[0117]

[0118] Comparative Example 13

[0119] Al-2.4Mg-1.86Mn alloy is currently available on the market.

[0120] Examples 17 to 20

[0121] Examples 17 to 20 are the same as Example 1 except that the parameters of the laser sintering in step (3) are different from those in Example 1.

[0122] The parameters of the laser sintering in step (3) are shown in Table 6.

[0123] Table 6:

[0124]

[0125] Note: “-” in the above table means “same as Example 1”.

[0126] Examples 21 to 24

[0127] Examples 21 to 24 are the same as Example 1 except that the parameters of the heat treatment in step (3) are different from those in Example 1.

[0128] The parameters of the heat treatment in step (3) are shown in Table 7.

[0129] Table 7:

[0130]

[0131]

[0132] Note: “-” in the above table means “same as Example 1”.

[0133] Experimental Example 1

[0134] In order to show that the aluminum alloy frame prepared in the present application has the effects of high strength and high toughness, and can effectively alleviate the problem of frame fracture of the existing traditional aluminum alloy frame photovoltaic module when loaded, the aluminum alloy frames prepared in Examples 1 to 16 of the present application and Comparative Examples 1 to 21 are now subjected to performance tests.

[0135] The specific method is as follows:

[0136] (1) Cut the sample into a cylindrical compression specimen with a diameter of 3 mm and a height of 6 mm using the wire cutting method, and remove the oxide film on both ends and the surface of the sample using sandpaper;

[0137] (2) Heat treatment of the samples at 350°C for different aging times;

[0138] (3) The heat-treated samples were subjected to compression tests using a universal testing machine with a compression speed set to 0.5 mm / min. The results showed that the compressive yield strength of the samples reached 560 MPa at 350°C-6h.

[0139] Note: To avoid the inconvenience caused by the excessive strength of the sample, this experimental example uses samples formed by laser sintering, cuts them, and then performs heat treatment testing.

[0140] (4) The sample was subjected to compression test using a universal testing machine with a compression speed set to 0.5 mm / min, and the compressive yield strength of the sample at 350°C-6h was obtained.

[0141] The specific test results are shown in Table 8 and Table 9:

[0142] Table 8:

[0143]

[0144]

[0145] Table 9:

[0146] Group Compression yield strength MPa Comparative Example 1 480 Comparative Example 2 490 Comparative Example 3 490 Comparative Example 4 470 Comparative Example 5 500 Comparative Example 6 520 Comparative Example 7 510 Comparative Example 8 530 Comparative Example 9 500 Comparative Example 10 520 Comparative Example 11 500 Comparative Example 12 520 Comparative Example 13 480

[0147] Table 10:

[0148] Group Compression yield strength MPa Embodiment 17 450 Embodiment 18 500 Embodiment 19 490 Embodiment 20 430 Embodiment 21 505 Embodiment 22 395 Embodiment 23 505 Embodiment 24 475

[0149] It can be seen from Tables 8 to 10 above that the aluminum alloy frames prepared in Examples 1 to 16 of the present application have better compressive yield strength than the existing traditional aluminum alloy frames in Comparative Example 13, among which: the aluminum alloy frame prepared in Example 1 has the best compressive yield strength, and its yield strength can reach 560 MPa after heat treatment.

[0150] Comparative Examples 1 to 4 Since the Al-Mg-Mn-Er-Zr alloy powder does not contain some alloy raw materials, the solid solution strengthening and second phase strengthening effects of the alloy samples will be weakened, affecting the yield strength of the alloy;

[0151] The Mg content in Comparative Example 5 is only 1%, which is less than the Mg1.5-4.6% embodiment in the present application. After the Mg content is reduced, the formation of the co-segregated phase of Zr, Mn, and Mg is reduced, and the solid solution effect is relatively poor. The Mg content in Comparative Example 6 is 5%, and the solid solution strengthening effect is better, but the compressive yield strength is still lower than the effect of 560MPa in the present application embodiment, indicating that in the present application alloy, at the composition content of "Mg2.74%, Mn6.01%, Er0.86%, Zr0.52%", each element has a better synergistic effect, and the prepared alloy has a higher compressive yield strength.

[0152] The content of Mn in Comparative Example 7 is only 3.5%, which is less than the implementation method of Mn 4.2-6.7% in the embodiment of the present application. After the reduction of Mn, the formation of the co-segregated phase of Zr, Mn and Mg is reduced, and the solid solution effect is relatively poor. While the content of Mn in Comparative Example 8 is 7.2%, the compressive yield strength is still lower than the effect of 560MPa in the embodiment of the present application, indicating that in the alloy of the present application, at the composition content of "Mg 2.74%, Mn 6.01%, Er 0.86%, Zr 0.52%", each element has a better synergistic effect, and the prepared alloy has a higher compressive yield strength.

[0153] The Er content in Comparative Example 9 is only 0.2%, which is less than the Er content of 0.4-2.8% in the embodiment of the present application. The Al3Er phase is reduced, so the mechanical properties are poor. The Er content in Comparative Example 10 is 3.5%, but the compressive yield strength is still lower than the effect of 560MPa in the embodiment of the present application, indicating that in the alloy of the present application, at the composition content of "Mg2.74%, Mn6.01%, Er0.86%, Zr0.52%, ", each element has a better synergistic effect, and the prepared alloy has a higher compressive yield strength.

[0154] The Zr content in Comparative Example 11 is only 0.1%, which is less than the Zr content of 0.3-1.6% in the embodiment of the present application. The reduction of Zr reduces the formation of the co-segregated phase of Zr, Mn, and Mg, and the solid solution effect is relatively poor. The Zr content in Comparative Example 12 is 2%, but the compressive yield strength is still lower than the effect of 560MPa in the embodiment of the present application, indicating that in the alloy of the present application, at the composition content of "Mg2.74%, Mn6.01%, Er0.86%, Zr0.52%, ", each element has a better synergistic effect, and the prepared alloy has a higher compressive yield strength.

[0155] The laser sintering parameters of Examples 17 to 20 are not within the range of Examples 1 to 16 of the present application. In Example 18, as the power increases, the sample forming quality is improved, thereby making the sample mechanical properties better; in Example 17, the power is reduced to 200W, and the sample mechanical properties are poor; in Examples 19 and 20, too low and too high scanning speeds will affect the sample forming quality, produce holes or incomplete melting defects, and affect the sample mechanical properties;

[0156] The heat treatment parameters of Examples 21 to 24 are not within the range of Examples 1 to 16 of the present application. Since the aging temperature of Examples 21 and 23 is too low and the aging time is too short, there are fewer solid solution elements in the samples, which makes the solid solution strengthening effect weaker and the mechanical properties are improved less. Since the aging temperature of Examples 22 and 24 is too high and the aging time is too long, the Al6Mn phase precipitated in the samples grows and coarsens, the strengthening effect is weakened, and the mechanical properties are reduced.

[0157] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An Al-Mg-Mn-Er-Zr alloy powder, characterized in that: The alloy powder comprises the following components in percentage by mass: Mg 1.5-4.6%, Mn 4.2-6.7%, Er 0.4-2.8%, Zr 0.3-1.6%, and the balance is Al.

2. The Al-Mg-Mn-Er-Zr alloy powder according to claim 1, characterized in that: The alloy powder comprises the following components by mass percentage: Mg 2-3%, Mn 5.5-6.5%, Er 0.4-1.2%, Zr 0.3-0.8%, and the balance is Al; Preferably, the alloy powder comprises the following components in percentage by mass: Mg 2.74%, Mn 6.01%, Er 0.86%, Zr 0.52%, and the balance is Al.

3. Use of the Al-Mg-Mn-Er-Zr alloy powder according to claim 1 or 2 in preparing an aluminum alloy frame for a photovoltaic module; Preferably, the aluminum alloy frame is a high-strength aluminum alloy frame, and the yield strength of the aluminum alloy frame is 480-560 MPa.

4. A method for preparing an aluminum alloy frame for a photovoltaic module, characterized in that: The preparation method comprises: The Al-Mg-Mn-Er-Zr alloy powder raw material according to claim 1 or 2 is weighed according to the component ratio, mixed to obtain a powder material; the powder material is subjected to laser melting metallization and molding to obtain an intermediate aluminum alloy frame; then laser sintering and curing heat treatment are sequentially performed to obtain an aluminum alloy frame for a photovoltaic module.

5. The method for preparing an aluminum alloy frame for a photovoltaic module according to claim 4, characterized in that: The laser melting metallization comprises: S1: According to the model data, the powder material A is laid into a single-layer powder bed using a powder spreader, and then the laser heat source scans the powder bed for melting to metalize the single-layer powder bed; S2: Repeat step S1 on the metallized single-layer powder bed until the Al-Mg-Mn-Er-Zr alloy frame is formed.

6. The method for preparing an aluminum alloy frame for a photovoltaic module according to claim 5, characterized in that: In the step S1, the powder material A is laid to form a single-layer powder bed with a thickness of 20 to 40 μm, preferably 30 μm.

7. The method for preparing an aluminum alloy frame for a photovoltaic module according to claim 5, characterized in that: The laser heat source power of the laser heat source scanning the powder bed in step S1 is 250-350W; And / or, in step S1, the laser scanning speed of the laser heat source scanning the powder bed is 800-1200 mm / s.

8. The method for preparing an aluminum alloy frame for a photovoltaic module according to claim 4, characterized in that: The laser sintering parameters satisfy at least one of the following: Laser power is 250-350W; Laser scanning speed is 800~1200mm / s; The laser scanning interval is 100 μm; The phase angle of laser sintering is 67°; The spot diameter of laser sintering is 75 μm.

9. The method for preparing an aluminum alloy frame for a photovoltaic module according to claim 4, characterized in that: The aging temperature of the curing heat treatment includes 100 to 500° C., and the aging treatment time includes 1 to 12 hours; Preferably, the aging temperature of the curing heat treatment is 320-350° C., and the aging treatment time is 2 hours.

10. An aluminum alloy frame for a photovoltaic module, characterized in that: The aluminum alloy frame is mainly prepared by the preparation method of the aluminum alloy frame according to any one of claims 4 to 9.

Citation Information

Patent Citations

  • Al-Mg-Sc-Zr series aluminum alloy composition for selective laser melting technology and preparation method for molding part

    CN108486433A

  • Al-Mg-Er-Zr serial aluminum alloy and preparation method

    CN109338182A

  • Method for improving formability of high-strength aluminum alloy powder for 3D printing

    CN111360257A

  • Alloy capable of being printed in 3D mode

    CN117042911A

  • Preparation method of heterostructure in 3D printed Al-Mg alloy

    CN117532013A