Method for preventing fracture of super duplex stainless steel plate blank

Through smelting component control and continuous casting cooling control, the problem of fracture of super duplex stainless steel slabs is solved, and the stability and material yield of the slabs are improved, reducing the risk of fracture.

CN119061309APending Publication Date: 2024-12-03ZHENSHI GROUP EASTERN SPECIAL STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411158427.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Super duplex stainless steel slabs are prone to break during storage and grinding, resulting in reduced material plasticity and concentrated internal stress, increasing the risk of fracture.

Method used

Through the control of smelting components, the mass fraction of sulfur element is less than 0.0015%, and the parallel section of the straightener is cooled by cooling water in the continuous casting process. After cutting the fire and putting it into a water tank for cooling. Combined with the blanking treatment and water cooling, the blanking is controlled. Cooling rate and temperature avoid precipitation of σ phase and reduce internal stress.

Benefits of technology

It effectively prevents slab fracture, improves product yield, and reduces personnel and equipment risks caused by fracture.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a method for preventing a super duplex stainless steel plate blank from being fractured, and belongs to the technical field of metal pressure machining. The method comprises the steps of smelting component control and continuous casting billet cooling control, wherein the mass fraction of the sulfur element in the steel is less than 0.0015%; in the continuous casting process, the specific water flow of secondary cooling water passing through a parallel section of a straightening machine is 0.3-0.4 L / Kg, the secondary cooling water is put into a water tank to be cooled after being cut into blocks through fire, and after being soaked in water to be cooled, the plate blank is lifted out of the water tank and placed in an open space to be stored; after the plate blank is cooled, cogging treatment is carried out, the soaking time of a heating furnace is 50-60 min, the tapping temperature is 1245-1265 DEG C, rough rolling is carried out for 4-5 passes, the swinging time of the plate blank on a roller way is not less than 10 min, the steel lifting temperature is 550-650 DEG C, the cogged plate blank is put into a water tank to be cooled, cooling is carried out for a certain time, the surface temperature center of the cooled plate blank is 200-4000 DEG C, and the plate blank is put in an open space after being lifted out. The super duplex stainless steel has no fracture phenomenon in the grinding and stockpiling periods, the product yield is improved, the personnel and equipment risks caused by fracture are reduced, and the use requirements are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method, in particular to a method for preventing super duplex stainless steel slab from breaking, and belongs to the technical field of metal pressure processing. Background Art

[0002] Super duplex stainless steel has ferrite and austenite coexisting in its microstructure at room temperature, with a duplex ratio close to 1:1. It has the advantages of both austenitic and ferritic stainless steels, high strength and good corrosion resistance, and is therefore widely used in industrial fields such as petrochemicals, salt production, and marine engineering. Super duplex stainless steel, with a pitting equivalent PREN>41, has outstanding advantages in harsh environments such as chloride ions and stress corrosion. Compared with ordinary duplex stainless steel, the content of Cr, Mo, and N in the steel is increased, and it has higher strength and better corrosion resistance.

[0003] The Chinese patent with the publication date of July 11, 2023 and the publication number of CN116411156A discloses an invention patent named "A high-strength and tough layered duplex stainless steel and its preparation method". The patent heats the two-phase layered stainless steel to between 1100℃-1200℃ and keeps it warm for 3h and then air cools it to room temperature to obtain an α phase and a highly stable γ phase; although the strength of the duplex steel prepared by the patent is increased by about 200MPa to 1300MPa, at the same time, the uniform elongation remains basically unchanged (18%), and the three-point bending cyclic loading experiment shows that the fracture toughness of the nano-scale B2 particle reinforced layered duplex steel prepared by this method can reach 176MPa·m1 / 2, but through the super duplex stainless steel of this application, no fracture phenomenon occurs, which can improve the product yield rate.

[0004] Compared with conventional duplex stainless steel, super duplex stainless steel has higher Cr, Mo and N content. The molten steel is very likely to precipitate brittle phases such as σ phase during the continuous casting solidification process. Austenite is a face-centered cubic structure, ferrite is a body-centered cubic structure, and σ phase is a body-centered tetragonal structure. The large amount of precipitation of σ phase will inevitably lead to an increase in the volume of the material, resulting in internal stress concentration and a significant reduction in the plasticity of the material. Under the combined effect of these two aspects, the slab is very likely to break during the storage and grinding process. Summary of the invention

[0005] The object of the present invention is to overcome the above-mentioned deficiencies in the prior art and to provide a method for preventing super duplex stainless steel slab fracture, which is easy to operate, can improve product yield, and reduce the risks to personnel and equipment caused by fracture.

[0006] The technical solution adopted by the present invention to solve the above problem is: the method for preventing super duplex stainless steel slab from breaking includes smelting component control and continuous casting slab cooling control, characterized in that the specific steps are as follows: (S1) Smelting composition control The mass fraction of sulfur in super duplex stainless steel is less than 0.0015%; the pitting equivalent PREN of super duplex stainless steel is greater than 41, PREN=1*Cr%+3.3*Mo%+20*N%; (S2) Continuous casting cooling control Super duplex stainless steel, during continuous casting, the specific water volume of the secondary cooling water in the parallel section of the straightener is 0.3-0.4L / Kg. After fire cutting and block cutting, the slab is placed in a water tank for cooling. After the slab is cooled by soaking in water, it is lifted out of the water tank and placed in an open space for storage. After the slab is cooled, it is opened. The heating furnace soaking period is 50-60min, the steel tapping temperature is 1245-1265℃, and after 4-5 rough rolling passes, the slab swings on the roller for no less than 10min, the hanging steel temperature is 550-650℃, and the opened slab is placed in a water tank for cooling. The cooling time is 10-20min. After cooling, the center temperature of the slab surface is 200-400℃. After the slab is lifted out, it is placed in an open space.

[0007] Preferably, the specific soaking step in step (S2) of the present invention is as follows: the slab is soaked in the water tank for 30-40 minutes, and the temperature of the slab after being cooled in the water tank is not higher than 400°C.

[0008] Preferably, in the continuous casting process of step (S2) of the present invention, the cross-section of the continuously cast billet is 220 mm.

[0009] Preferably, in the blanking process of the present invention, the soaking time in the heating furnace is 53 minutes and the tapping temperature is 1254°C.

[0010] Preferably, the slab opening process of the present invention is performed four times, the slab swings on the roller table for no less than 10 minutes, and the hanging steel temperature is 580°C.

[0011] Preferably, the slab after blanking in the present invention is placed in a water tank for cooling, and the cooling time is 14 minutes.

[0012] Preferably, after the slabs of the present invention are water-cooled and lifted out of the water tank, they are not stacked for storage.

[0013] Preferably, the super duplex stainless steel of the present invention is S32750.

[0014] Compared with the prior art, the present invention has the following advantages and effects: no fracture occurs during the grinding and storage of super duplex stainless steel S32750, thereby improving the product yield rate and reducing the risks to personnel and equipment caused by fracture. DETAILED DESCRIPTION

[0015] The present invention will be further described in detail below in conjunction with the embodiments. The following embodiments are for explanation of the present invention but the present invention is not limited to the following embodiments.

[0016] The method for preventing super duplex stainless steel slab from breaking in this embodiment includes smelting composition control and continuous casting slab cooling control, and is characterized in that the specific steps are as follows: (S1) Smelting composition control The mass fraction of sulfur in super duplex stainless steel is less than 0.0015%; the pitting equivalent PREN of super duplex stainless steel is greater than 41, PREN=1*Cr%+3.3*Mo%+20*N%.

[0017] (S2) Continuous casting cooling control Super duplex stainless steel, during continuous casting, the specific water volume of the secondary cooling water in the parallel section of the straightener is 0.3-0.4L / Kg (to increase the cooling rate). After fire cutting, the blocks are placed in a water tank for cooling. After the slabs are cooled in water, they are lifted out of the water tank and placed in an open space for storage. After the slab is cooled, it is opened. The heating furnace soaking period is 50-60min, the steel tapping temperature is 1245-1265℃, and after 4-5 rough rolling passes, the slab swings on the roller for no less than 10min, the hanging steel temperature is 550-650℃, and the opened slab is placed in a water tank for cooling. The cooling time is 10-20min. After cooling, the center temperature of the slab surface is 200-400℃. After the slab is lifted out, it is placed in an open space.

[0018] The specific soaking steps in step (S2) are as follows: the slab is soaked in the water tank for 30-40 minutes, and the temperature of the slab taken out after being cooled in the water tank is not higher than 400°C.

[0019] During the continuous casting process of step (S2), the cross section of the continuous casting billet is 220 mm.

[0020] The super duplex stainless steel in this embodiment is first subjected to a blanking process before the subsequent rolling process.

[0021] In this embodiment, the super duplex stainless steel slabs are not stacked for storage after being water-cooled and lifted out of the water tank.

[0022] The super duplex stainless steel in this embodiment is S32750. After the continuous casting slab is cut, it is hoisted into a cooling water tank to increase the cooling rate and achieve rapid cooling.

[0023] Example 1: The super duplex stainless steel S32750, during the continuous casting process, has a specific water volume of 0.311L / Kg in the parallel section of the straightening machine. After the fire cutting, it is placed in a water tank for cooling. The slab is soaked in the water tank for 30 minutes. The temperature of the slab after cooling in the water tank is 210°C. After the slab is water-cooled, it is lifted out of the water tank and placed in an open space for storage. After the slab is cooled, it is opened for processing. The heating furnace soaking time is 53 minutes, the steel tapping temperature is 1254°C, and after 4 rough rolling passes, the roller swing time is 10 minutes, and the steel hanging temperature is 580°C. The slab after opening is placed in a water tank for cooling. The cooling time is 14 minutes. After cooling, the surface temperature of the slab is about 300°C. After the slab is lifted out, it is placed in an open space. After the slab is treated in the above manner, the surface is overall flat, without surface cracks and edge cracks, and the overall effect is good.

[0024] Example 2: The super duplex stainless steel S32750, during the continuous casting process, has a water volume ratio of 0.311L / Kg in the parallel section of the straightener, is fire-cut into blocks, and is placed in a water tank for cooling. The slab is soaked in the water tank for 30 minutes, and the temperature of the slab after cooling in the water tank is 235°C. After the slab is water-cooled, it is hoisted out of the water tank and placed in an open space for storage; after the slab is cooled, it is opened for processing, the soaking time in the heating furnace is 53 minutes, the steel tapping temperature is 1255°C, and after 4 rough rolling passes, the roller swing time is 10 minutes, the steel hanging temperature is 590°C, and the opened slab is placed in a water tank for cooling, the cooling time is 15 minutes, and the surface temperature of the slab after cooling is about 300°C in the center. After the slab is hoisted out, it is placed in an open space. The slab has a flat shape, no surface cracks or edge cracks, and the overall effect is good.

[0025] Through the above description, those skilled in the art can already implement it.

[0026] In addition, it should be noted that the shapes and names of the parts and components of the specific embodiments described in this specification may be different, and the above content described in this specification is only an example of the structure of the present invention. All equivalent changes or simple changes made based on the structure, features and principles described in the patent concept of the present invention are included in the protection scope of the patent of the present invention. Technicians in the technical field to which the present invention belongs can make various modifications or supplements to the specific embodiments described or replace them in a similar manner, as long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preventing super duplex stainless steel slab from breaking, comprising smelting composition control and continuous casting slab cooling control, characterized in that: The specific steps are as follows: (S1) Smelting composition control The mass fraction of sulfur in super duplex stainless steel is less than 0.0015%; the pitting equivalent PREN of super duplex stainless steel is greater than 41, PREN=1*Cr%+3.3*Mo%+20*N%; (S2) Continuous casting cooling control Super duplex stainless steel, during continuous casting, the specific water volume of the secondary cooling water in the parallel section of the straightener is 0.3-0.4L / Kg. After fire cutting and block cutting, the slab is placed in a water tank for cooling. After the slab is cooled by soaking in water, it is lifted out of the water tank and placed in an open space for storage. After the slab is cooled, it is opened. The heating furnace soaking period is 50-60min, the steel tapping temperature is 1245-1265℃, and after 4-5 rough rolling passes, the slab swings on the roller for no less than 10min, the hanging steel temperature is 550-650℃, and the opened slab is placed in a water tank for cooling. The cooling time is 10-20min. After cooling, the center temperature of the slab surface is 200-400℃. After the slab is lifted out, it is placed in an open space.

2. The method for preventing super duplex stainless steel slab from fracture according to claim 1, characterized in that: The specific soaking steps in the step (S2) are as follows: the slab is soaked in the water tank for 30-40 minutes, and the temperature of the slab after being cooled in the water tank is not higher than 400°C.

3. The method for preventing super duplex stainless steel slab from fracture according to claim 1, characterized in that: During the continuous casting process of step (S2), the cross section of the continuous casting billet is 220 mm.

4. The method for preventing super duplex stainless steel slab from fracture according to claim 1, characterized in that: The billet is opened and the soaking time in the heating furnace is 53 minutes, and the steel-out temperature is 1254℃.

5. The method for preventing super duplex stainless steel slab from fracture according to claim 1, characterized in that: The slab is opened for 4 times, the slab swings on the roller for no less than 10 minutes, and the hanging steel temperature is 580℃.

6. The method for preventing super duplex stainless steel slab from fracture according to claim 1, characterized in that: The slab after opening is placed in a water tank for cooling, and the cooling time is 14 minutes.

7. The method for preventing super duplex stainless steel slab from fracture according to claim 1, characterized in that: After the slabs are water-cooled, they are lifted out of the water tank and stored without stacking.

8. The method for preventing super duplex stainless steel slab from fracture according to claim 1, characterized in that: The super duplex stainless steel is S32750.