Method for presetting gold-tin solder
The multi-target sputtering system controls the sputtering parameters and sample stage rotation of gold tin solder, and prepares high-quality gold tin solder with a gold-out mass ratio of 8% to 12%, which solves the high cost of gold tin solder in the prior art and The problem of poor welding quality has achieved cost reduction and improved welding performance.
Patent Information
- Application Number
- CN202411166659.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
AI Technical Summary
The existing gold-tin solder has problems of alignment accuracy and high cost during the soldering process, especially in the assembly of high-end optical chips, and it is difficult to achieve the preparation of gold-tin solder with a gold-mass ratio below 10%.
Using a multi-target sputtering system, by controlling the sputtering power and rate of the gold target and multiple tin targets, combined with high-speed rotation of the sample table, gold tin solder with a gold mass ratio of 8% to 12%, which reduces the Preparation cost of gold-tin solder and improve soldering quality.
The cost of gold-tin solder is significantly reduced, the soldering quality and uniformity are improved, and the uniformity of the gold-tin film layer is strictly controlled within ±2%, meeting the soldering needs of high-end optical chips.
Smart Images

Figure CN119061360A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chip welding, and in particular relates to a method for pre-setting gold-tin solder. Background Art
[0002] In optical modules, the welding of optical chips is crucial to the transmission of optical performance. Conventional gold-tin solder sheets cannot meet the requirements of optical device assembly batch production in terms of welding alignment accuracy and solder sheet size. Currently, the alignment accuracy problem is mainly solved by pre-setting gold-tin solder on the substrate. The pre-setting technology of gold-tin solder is a key process in the field of electronic assembly. There are many methods, each with its own characteristics. The most commonly used methods are electroplating and physical vapor deposition.
[0003] Among them, the electroplating method is to configure the plating solution with gold salt and tin salt in a certain proportion, and deposit it on the substrate by electroplating. It has the advantages of low cost and mass production. However, the uniformity of the gold-tin mass ratio of electroplated gold-tin solder is poor, and it depends greatly on the stability of the plating solution. The produced gold-tin solder is difficult to be used in the welding of high-end optical chips. The physical vapor deposition method is to deposit gold-tin alloy evaporation particles or alloy targets on the substrate by atomic deposition through evaporation or sputtering. However, due to the obvious difference in the atomic weight of Au and Sn, the mass ratio of Au and Sn deposited on the substrate is prone to uncontrollable problems. At the same time, the gold mass ratio of the currently used gold-tin solder is 70-80%, the gold mass ratio is high, and the material cost is expensive, which also restricts the large-scale application of pre-set gold-tin solder. The co-evaporation process can reduce the mass ratio of gold in gold-tin solder to a certain extent, but it is very limited. To prepare gold-tin solder with a gold mass ratio of less than 10%, there must be a very large difference between the film formation rates of Au and Sn. For example, in a gold-tin solder with a gold mass ratio of 10%, the tin film formation rate must be 27.2 times that of the gold film formation rate. The conventional co-evaporation process is limited by the power limit of the electron beam and cannot meet the above requirements. In addition, the preparation of Au-Sn alloy solder by magnetron co-sputtering can make gold and tin evenly mixed, achieve precise adjustment of their mass ratio, and improve welding quality, but the mass proportion of gold is still very high, and it is difficult to prepare a gold-tin solder with a gold mass ratio of about 10%. Summary of the invention
[0004] In view of this, the primary purpose of the present invention is to provide a method for pre-setting gold-tin solder, in which the gold-tin solder is prepared by adopting a multi-target sputtering system, the gold target and multiple tin targets are controlled to be sputtered simultaneously, and the sputtering power is coordinated and the sputtering rate is adjusted to prepare the gold-tin solder with a gold mass ratio of 8% to 12%, thereby greatly reducing the preparation cost of the gold-tin solder.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention first provides a method for pre-setting gold-tin solder, the key step of which is gold-tin co-sputtering. The gold-tin co-sputtering process is as follows:
[0007] A multi-target co-sputtering process is adopted to control the simultaneous sputtering of one gold target and three to four tin targets, wherein the sputtering power of the gold target is 400 to 800 W, and the sputtering rate is 0.2 to 0.3 nm / s; the sputtering power of each tin target is 1500 to 2500 W, and the sputtering rate is 0.9 to 2.1 nm / s; and during the co-sputtering process, the sample stage rotates at a high speed of 2 to 10 s / rev.
[0008] The multi-target co-sputtering process described herein is implemented by using a multi-target sputtering system well known in the art. The specific number of targets can be selected according to needs. For example, in one embodiment of the present invention, a vertical six-target sputtering system is used, and the target positions and sample stages in the chamber are distributed as follows: Figure 1 As shown in .
[0009] During the specific operation, one target position is set to place the gold target, and 3 to 4 target positions are set to place the tin target. During the co-sputtering preparation process of the gold-tin solder, one gold target and multiple tin targets are sputtered simultaneously, and the sputtering power and sputtering rate are adjusted to control the gold-tin film formation rate, thereby preparing a gold-tin solder with a gold mass ratio of 8% to 12%.
[0010] Among them, the sputtering power of the gold target is 400-800 W, for example, it can be 400 W, 500 W, 600 W, 700 W or 800 W; the sputtering rate of the gold target is 0.1-0.3 nm / s, for example, it can be 0.1 nm / s, 0.15 nm / s, 0.2 nm / s, 0.25 nm / s or 0.3 nm / s.
[0011] The sputtering power of each tin target is 1500-2500 W, for example, it can be 1500 W, 1600 W, 1700 W, 1800 W, 1900 W, 2000 W, 2100 W, 2200 W, 2300 W, 2400 W or 2500 W; the sputtering rate of each tin target is 0.9-2.1 nm / s, for example, it can be 0.9 nm / s, 1.2 nm / s, 1.4 nm / s, 1.6 nm / s, 1.8 nm / s, 2.1 nm / s.
[0012] In addition, during the gold-tin co-sputtering process, the sample stage is controlled to rotate at a high speed, wherein the rotation speed is 2 to 10 s / rev, for example, 2 s / rev, 4 s / rev, 5 s / rev, 8 s / rev or 10 s / rev. The high-speed rotation of the sample stage can ensure that Au and multiple Sn target atoms are fully fused after sputtering, thereby avoiding local tin enrichment in the gold-tin film layer, and the gold-tin film layer deposited on the substrate has very good uniformity, and its uniformity can be strictly controlled within ±2%.
[0013] The above process can produce high-quality gold-tin solder with a gold mass ratio of 8% to 12%, significantly reducing the cost of gold-tin solder (compared to a gold mass ratio of 70% to 80%, the cost can be reduced by about 600%). It can be understood that the specific target position design, the sputtering power of the target material, the sputtering rate, and the rotation speed of the sample stage can all be designed according to the specific required gold content and gold-tin content.
[0014] The thickness of the gold-tin solder can be selected according to product requirements. In some specific embodiments of the present invention, the total thickness of the gold-tin solder is 3 to 8 μm.
[0015] According to a further solution, in the present invention, before the step of gold-tin co-sputtering, an oxygen plasma cleaning step is introduced to clean the surface of the substrate using oxygen as a process gas, thereby effectively increasing the adhesion between the metallization pattern and the subsequently formed solder resist layer, thereby improving product performance.
[0016] It is understandable that specific process parameters can be selected according to needs. In some specific embodiments of the present invention, the process parameters of oxygen plasma cleaning are: oxygen flow rate of 150-300 sccm, plasma excitation power of 200-400 W, and cleaning time of 2 min to 10 min.
[0017] It should be noted that the method for pre-depositing gold-tin solder in the present invention also includes a process for forming a metallization pattern, a solder mask layer, etc. on a substrate, which can be selected according to the needs of a process well known to those skilled in the art. In a specific embodiment of the present invention, the method for pre-depositing gold-tin solder includes the following steps:
[0018] S1. Provide a substrate.
[0019] The substrate described herein mainly refers to a ceramic substrate, and specific examples include an aluminum oxide substrate, an aluminum nitride substrate, or a silicon nitride substrate, but are not limited thereto. The substrate needs to be cleaned before use to ensure the cleanliness of the substrate. The specific cleaning method is a conventional method in the art and will not be described here.
[0020] S2. Forming a metallization pattern on the surface of the substrate.
[0021] The metallization pattern described in this article is a composite film layer, mainly including an adhesion layer, a first solder resist layer and a gold layer. Among them, the adhesion layer is one of Ti, WTi, NiCr, and TaN, and / or the first solder resist layer is at least one of Ni, Pt, and Pd. The film thickness of each layer can be designed as needed. In some specific implementation cases of the present invention, the thickness of the adhesion layer is 0.05-0.2 μm; and / or the thickness of the first solder resist layer is 0.05-0.2 μm; and / or the thickness of the gold layer is 0.5-5 μm. The specific metallization pattern formation process can be prepared by conventional means in the art such as cleaning, sputtering, electroplating, photolithography, etc. to obtain a metallization pattern as a bottom layer of gold-tin solder, which will not be specifically described here. It should be noted that after the metallization pattern is formed, high-temperature annealing is required to release the stress between the composite film layers. In a specific embodiment of the present invention, the high-temperature annealing process is vacuum baking at 300-400°C for 2-4 hours, and then naturally cooled to room temperature.
[0022] S3, preparing a gold-tin solder mask on the surface of the metallization pattern to expose the area where the gold-tin solder needs to be pre-placed.
[0023] Specifically, in step S3, a mask of gold-tin solder is prepared on the surface of the metallized pattern to expose the area where the gold-tin solder needs to be pre-placed. The mask can be prepared by a negative resist photolithography process well known in the art, including negative resist spinning, exposure, development and post-baking processes, to expose the area where the gold-tin solder needs to be pre-placed, and to cover the area where the gold-tin solder does not need to be processed with negative resist.
[0024] S4. Clean the substrate using an oxygen plasma cleaning process.
[0025] Through the oxygen plasma cleaning process, oxygen is used as the process gas to clean the substrate surface and remove the residual developer and water vapor in the mask making process, thereby effectively increasing the adhesion between the bottom metallization pattern and the subsequent film-forming solder mask layer, ensuring that the welding shear force meets the standard requirements. The specific oxygen plasma cleaning process can be carried out as described above.
[0026] S5. Place the substrate in a multi-target sputtering system to perform sputtering to form a second solder resist layer.
[0027] The solder resist layer may be made of conventional Ni, Pt, etc. in the art. Preferably, in the present invention, the second solder resist layer is configured as a Ni layer, thereby reducing the preparation cost of the solder resist layer. Preferably, the target material and adhesive material such as Ti of the second solder resist layer are placed at other target positions except for gold and tin, and a corresponding baffle is configured after the second solder resist layer is sputtered to avoid mutual contamination between the target materials. For details, see Figure 2The sputtering power of the Ni layer is 600-1500 W, the sputtering rate is 0.5-1 nm / s, and the sputtering thickness is 0.5-2 μm.
[0028] S6. Perform gold-tin co-sputtering on the surface of the second solder resist layer to form gold-tin solder.
[0029] Please refer to Figure 2 The arrangement in the embodiment is used to perform gold-tin co-sputtering. The specific steps and parameters can refer to those described above. The gold mass ratio of the gold-tin solder sputtered by this method is between 8% and 12%, and the film has excellent uniformity.
[0030] S7. Form a protective layer on the surface of the gold-tin solder.
[0031] After the gold-tin sputtering is completed, a protective layer is sputtered on the surface of the gold-tin solder. In the present invention, the protective layer is a gold layer, thereby effectively protecting the gold-tin solder from being oxidized in the environment. In some specific embodiments of the present invention, the thickness of the protective layer is 0.03-0.05 μm.
[0032] S8, removing the gold-tin solder mask to obtain a ceramic substrate with gold-tin solder pre-set.
[0033] The specific removal process can be performed in a manner well known in the art. For example, if the mask is formed using a negative resist photolithography process, the degumming process can be performed by soaking in a degumming solution at 80° C. for 30 minutes and then ultrasonicating at room temperature for 10 minutes.
[0034] The final structure of the ceramic substrate with pre-set gold-tin solder is as follows Figure 3 As shown in , a metallization pattern 2, a second solder resist layer 3, a gold-tin solder 4 and a protective layer 5 are sequentially formed on a substrate 1.
[0035] In addition, it should be noted that the purity of the target materials used in the present invention is 99.99% or more.
[0036] Beneficial effects of the present invention:
[0037] The present invention adopts a multi-target sputtering system to complete the preparation of the gold-tin film layer in one chamber, and obtains a gold-tin solder with a gold mass ratio of 8% to 12% by controlling the sputtering power and the sputtering rate, thereby significantly reducing the preparation cost of the preset gold-tin solder.
[0038] In addition, during the co-sputtering process, the sample stage rotates at high speed, so that the gold-tin film layer deposited on the substrate is of high quality, and the uniformity is strictly controlled within ±2%, so that a high-quality gold-tin film layer can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1This is a top view of the distribution of target positions inside the chamber of a vertical six-target sputtering system used in a preferred embodiment of the present invention.
[0040] Figure 2 This is a top view of the distribution of each target position during the gold-tin solder presetting process in Example 1.
[0041] Figure 3 The figure is a schematic diagram of the structure of the gold-tin solder prepared in a preferred embodiment of the present invention.
[0042] In the figure: 1-substrate, 2-metallization pattern, 3-second solder mask, 4-gold-tin solder, 5-protective layer. DETAILED DESCRIPTION
[0043] Embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. In addition, unless otherwise specified, methods that do not specifically record conditions or steps are conventional methods, and the reagents and materials used can be obtained from commercial sources.
[0045] Example 1
[0046] This embodiment provides a method for pre-setting gold-tin solder, and the specific steps are as follows:
[0047] a. Choose a clean 98% aluminum nitride ceramic substrate;
[0048] b. Using conventional thin film technology, a composite film system of WTi0.1μm / Ni0.5μm / Au3μm from bottom to top on the substrate surface is prepared as the bottom metallization pattern;
[0049] c. Perform annealing treatment on the metallized pattern by vacuum baking at 350° C. for 2 hours.
[0050] d. Use negative photolithography to prepare a gold-tin solder pattern mask;
[0051] e. The substrate is cleaned by plasma cleaning process, the process gas is 150sccm oxygen, the plasma excitation power is 300W, and the cleaning time is 5min;
[0052] f. Place the cleaned substrate Figure 1 The vertical six-target sputtering system shown in Figure 2The target materials are arranged at each target position, and the second solder resist layer is sputtered, which is a composite film layer of Ti0.1μm / Ni0.8μm from bottom to top;
[0053] g. A co-sputtering process was adopted to obtain a gold-tin solder with a gold mass ratio of 10% by evaporation by controlling the sputtering power of Au and Sn. Among them, the sputtering power of each of the three tin targets was 2450 W, and the sputtering rate was 1.98 nm / s. The sputtering power of one gold target was 600 W, and the sputtering rate was 0.25 nm / s. The total thickness of the sputtered gold-tin solder was 4 μm, and the co-sputtering time was 646 s. During the co-sputtering process, the sample stage rotated at a high speed of 5 s / rev.
[0054] h. Evaporate a 0.05 μm gold layer on the surface of 4 μm gold-tin solder at a sputtering rate of 0.5 nm / s;
[0055] i. Soak the evaporated substrate in a degumming solution at 80°C for 30 minutes and then ultrasonicate it at room temperature for 10 minutes. After removing the negative resist, scribing and graining with a grinding wheel is performed to obtain a ceramic substrate with pre-set gold-tin solder.
[0056] The welding performance of the ceramic substrate pre-set with gold-tin solder obtained in this embodiment was evaluated, wherein the welding process curve was: first preheating at 150°C for 15s, then heating to 240°C within 5s, maintaining at 240°C for 10s, and finally reducing to 150°C for 20s.
[0057] Using the above welding process curve to weld 5 chips with a size of 1mm×1mm, the measured welding shear thrust was 2.3~2.8kg, which meets the chip shear strength requirements of GJB548C-2021 method 2019.3 (≥1.2kg).
[0058] Example 2
[0059] This embodiment provides another method for pre-setting gold-tin solder, and the specific steps are as follows:
[0060] Steps a to d are the same as in Example 1.
[0061] e. The substrate is cleaned by plasma cleaning process, the process gas is 200 sccm oxygen, the plasma excitation power is 200 W, and the cleaning time is 10 min;
[0062] f. Place the cleaned substrate on a vertical six-target sputtering system to sputter the second solder resist layer, which is a composite film layer of Ti0.1μm / Ni0.8μm from bottom to top;
[0063] g. A co-sputtering process was adopted to obtain a gold-tin solder with a gold mass ratio of 8% by evaporation by controlling the sputtering power of Au and Sn. Among them, the sputtering power of each of the four tin targets was 2000 W, and the sputtering rate was 1.67 nm / s. The sputtering power of one gold target was 425 W, and the sputtering rate was 0.22 nm / s. The total thickness of the sputtered gold-tin solder was 6 μm, and the co-sputtering time was 869 s. During the co-sputtering process, the sample stage rotated at a high speed of 3 s / rev.
[0064] Steps h to i are the same as in Example 1.
[0065] The welding performance of the ceramic substrate pre-set with gold-tin solder obtained in this embodiment was evaluated, wherein the welding process curve was: first preheating at 150°C for 40s, then heating to 250°C within 5s, maintaining at 250°C for 5s, and finally reducing to 150°C for 20s.
[0066] Using the above welding process curve to weld 5 chips with a size of 1mm×1mm, the measured welding shear thrust was 1.7~2.4kg, which meets the chip shear strength requirements of GJB548C-2021 method 2019.3 (≥1.2kg).
[0067] Example 3
[0068] This embodiment provides a method for pre-setting gold-tin solder, and the specific steps are as follows:
[0069] a. Choose a clean 99.6% alumina ceramic substrate;
[0070] Steps b to d are the same as in Example 1.
[0071] e. The substrate is cleaned by plasma cleaning process, the process gas is 300 sccm oxygen, the plasma excitation power is 400 W, and the cleaning time is 2 min;
[0072] f. Place the cleaned substrate in a vertical six-target sputtering system to sputter the second solder resist layer, which is a composite film layer of Ti0.1μm / Ni1μm from bottom to top;
[0073] g. A co-sputtering process was adopted to obtain a gold-tin solder with a gold mass ratio of 12% by evaporation by controlling the sputtering power of Au and Sn. Among them, the sputtering power of each of the four tin targets was 1650 W, and the sputtering rate was 1.35 nm / s. The sputtering power of one gold target was 750 W, and the sputtering rate was 0.28 nm / s. The total thickness of the sputtered gold-tin solder was 5 μm, and the co-sputtering time was 876 s. During the co-sputtering process, the sample stage rotated at a high speed of 8 s / rev.
[0074] Steps h to i are the same as in Example 1.
[0075] The welding performance of the ceramic substrate pre-set with gold-tin solder obtained in this embodiment was evaluated, wherein the welding process curve was: first preheating at 150°C for 30s, then heating to 250°C within 5s, maintaining at 250°C for 5s, and finally reducing to 150°C for 20s.
[0076] Using the above welding process curve to weld 5 chips with a size of 1mm×1mm, the measured welding shear thrust was 2.0~2.6kg, which meets the chip shear strength requirements of GJB548C-2021 method 2019.3 (≥1.2kg).
[0077] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0078] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for pre-setting gold-tin solder, characterized in that: The process includes the steps of gold-tin co-sputtering, wherein the gold-tin co-sputtering process is as follows: A multi-target co-sputtering process is adopted to control the simultaneous sputtering of one gold target and three to four tin targets, wherein the sputtering power of the gold target is 400 to 800 W, and the sputtering rate is 0.2 to 0.3 nm / s; the sputtering power of each tin target is 1500 to 2500 W, and the sputtering rate is 0.9 to 2.1 nm / s; and during the co-sputtering process, the sample stage rotates at a high speed of 2 to 10 s / rev.
2. The method for pre-disposing gold-tin solder according to claim 1, characterized in that: The total thickness of the gold-tin solder is 3 to 8 μm.
3. The method for pre-disposing gold-tin solder according to claim 1, characterized in that: Before the step of gold-tin co-sputtering, an oxygen plasma cleaning step is included; Preferably, the process parameters of the oxygen plasma cleaning are: oxygen flow rate of 150-300 sccm, plasma excitation power of 200-400 W, and cleaning time of 2 min to 10 min.
4. The method for pre-placement of gold-tin solder according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: providing a substrate; forming a metallization pattern on a surface of a substrate; Prepare a gold-tin solder mask on the surface of the metallized pattern to expose the area where the gold-tin solder needs to be pre-placed; Cleaning the substrate using an oxygen plasma cleaning process; Placing the substrate in a multi-target sputtering system to perform sputtering to form a second solder resist layer; Performing gold-tin co-sputtering on the surface of the second solder resist layer to form gold-tin solder; Forming a protective layer on the surface of the gold-tin solder; The gold-tin solder mask is removed to obtain a ceramic substrate with gold-tin solder pre-applied thereon.
5. The method for pre-disposing gold-tin solder according to claim 4, characterized in that: The substrate is a ceramic substrate, and the ceramic substrate is an aluminum oxide substrate, an aluminum nitride substrate or a silicon nitride substrate.
6. The method for pre-disposing gold-tin solder according to claim 4, characterized in that: The metallization pattern is a composite film layer, including an adhesion layer, a first solder resist layer and a gold layer; Preferably, the adhesion layer is one of Ti, WTi, NiCr, and TaN; and / or the first solder resist layer is at least one of Ni, Pt, and Pd; Preferably, the thickness of the adhesion layer is 0.05 to 0.2 μm; and / or the thickness of the first solder resist layer is 0.05 to 0.2 μm; and / or the thickness of the gold layer is 0.5 to 5 μm.
7. The method for pre-disposing gold-tin solder according to claim 4, characterized in that: After the metallization pattern is formed, high temperature annealing is required. The high temperature annealing process is vacuum baking at 300-400°C for 2-4 hours and then naturally cooling to room temperature.
8. The method for pre-disposing gold-tin solder according to claim 4, characterized in that: The gold-tin solder mask is prepared using a negative photolithography process.
9. The method for pre-disposing gold-tin solder according to claim 4, characterized in that: The second solder resist layer is a Ni layer, the sputtering power of the Ni layer is 600-1500W, the sputtering rate is 0.5-1nm / s, and the sputtering thickness is 0.5-2μm.
10. The method for pre-disposing gold-tin solder according to claim 4, characterized in that: The protective layer is a gold layer, and its thickness is 0.03-0.05 μm.