Method for manufacturing anti-sticking film on mold with nano structure
By using oxygen-containing plasma pretreatment and PEALD technology to deposit anti-staining mucosa on nanostructured molds, the problem of insufficient service life of the mold is solved, and the generation of anti-staining mucosa with uniform thickness and high adhesion is achieved, which improves the service life of the mold. and transfer times.
Patent Information
- Application Number
- CN202310825641.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2023-07-06
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, when using nanostructured molds, the method of forming anti-stic mucosa has difficulties in controlling the film thickness, the risk of damage to the plating by wet solvents, and the film thickness unevenness on the nanostructures, resulting in insufficient service life of the mold.
The anti-distance mucosa is deposited on the nanostructure surface by oxygen-containing plasma pretreatment and plasma-assisted atomic layer deposition (PEALD). By introducing oxygen-containing plasma and carbon-silicon long-chain compound precursors, a uniform anti-distance mucosa is formed, which improves the Adhesion and reactivity.
The uniform thickness of anti-stic film is achieved on the nanostructured mold, which improves the anti-stic properties and service life of the mold, and ensures efficient transfer times and adhesion.
Smart Images

Figure CN119061377A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing an anti-adhesive film, in particular to a method for manufacturing an anti-adhesive film on a mold with a nanostructure. Background Art
[0002] Nanoimprint lithography (NIL) is a simple, reliable and cost-effective lithography technology, and has attracted much attention from the industry. NIL uses a mold (stamp) formed with a nanostructure to heat a polymer (such as a photoresist layer) on a substrate to a temperature above its glass transition temperature and then apply pressure to transfer the pattern of the nanostructure to the photoresist layer on the substrate. In this way, it can replicate nano patterns multiple times and achieve a high resolution of up to 10nm, and has a higher yield than processing methods such as electron beam or scanning probe microscopy (SPM) lithography.
[0003] An existing NIL is Figure 1 As shown, it includes a step (A), a step (B), and a step (C) in sequence. Specifically, when a transfer process is performed on a mold 11 having a nanostructure 111, the nanostructure 111 on the mold 11 will produce adhesion with a photoresist layer 13 on a substrate 12. Therefore, it is necessary to prepare an anti-adhesion film 14 on the mold 11 having the nanostructure 111 to reduce the risk of adhesion between the nanostructure 111 and the photoresist layer 13, thereby increasing the service life of the mold 11.
[0004] The common method of forming an anti-adhesive film is to make a self-assembled monolayer (SAM) by immersion. The disadvantage of the SAM is that the film thickness is difficult to control and the plated object needs to be immersed in a wet solvent environment, which may damage the plated object.
[0005] In addition, physical vapor deposition (PVD) and chemical vapor deposition (CVD) are also common methods for making anti-adhesive films. However, for objects or molds with nanostructures, PVD and CVD have poor uniformity in film thickness due to the high aspect ratio of the nanostructures. Although the film can be removed smoothly after transfer, it is easy to cause inconsistency in the morphology of the transferred nanostructures.
[0006] From the above description, it can be seen that improving the method of making an anti-sticking film on a mold with a nanostructure to solve the problem of insufficient mold service life is a topic that needs to be broken through by relevant technical personnel in the technical field to which this case belongs. Summary of the invention
[0007] The object of the present invention is to provide a method for preparing an anti-adhesive film on a mold having a nanostructure, which can solve the problem of insufficient mold service life.
[0008] The method for making an anti-adhesive film on a mold having a nanostructure of the present invention comprises the following steps: step (a), and step (b).
[0009] The step (a) is to pre-treat the mold by applying oxygen-containing plasma, and the surface of the mold has a nanostructure.
[0010] The step (b) is to deposit an anti-adhesive film on the surface of the nanostructure by plasma enhancement atomic layer deposition (PEALD) in a reaction chamber provided with the mold after the step (a). The step (b) has the following sub-steps in sequence: sub-step (b1), sub-step (b2), sub-step (b3), and sub-step (b4).
[0011] The step (b1) is to introduce oxygen-containing plasma into the reaction chamber and immerse the mold in the oxygen-containing plasma to form a plurality of dangling bonds on the surface of the nanostructure.
[0012] The sub-step (b2) is to clear the oxygen-containing plasma in the reaction chamber.
[0013] The step (b3) is to introduce a precursor into the reaction chamber and immerse the mold in the precursor to react with the dangling bonds on the surface of the nanostructure and produce by-products, thereby forming the anti-adhesive film on the surface of the nanostructure.
[0014] The sub-step (b4) is to remove by-products in the reaction chamber.
[0015] In the present invention, the precursor is a carbon-silicon long-chain compound with a carbon number between 3 and 20.
[0016] The method for making an anti-adhesive film on a nanostructured mold of the present invention comprises a carbon chain of the carbon-silicon long-chain compound having a halogen, and a functional group capable of undergoing a hydrolysis-condensation reaction on the silicon base.
[0017] In the method for making an anti-adhesive film on a nanostructured mold of the present invention, the carbon-silicon long-chain compound is selected from 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, 1H, 1H, 2H, 2H-perfluorodecyltrichlorosilane, octadecyltrichlorosilane, or dimethyldichlorosilane.
[0018] The method for making an anti-adhesive film on a mold with a nanostructure of the present invention is made of a material selected from polymers, metals, semiconductors, ceramics, or glass.
[0019] The method for making an anti-adhesive film on a mold with a nanostructure of the present invention, wherein the nanostructure of the mold is selected from nanopores, nanopillars, or nanogrooves, and the aspect ratios of the nanopores, nanopillars, and nanogrooves are all between 1.7 and 10.
[0020] In the method for making an anti-adhesive film on a mold with a nanostructure, the sizes of the nanopores, nanocolumns and nanogrooves are all between 50nm and 400nm.
[0021] In the method for making an anti-adhesive film on a nanostructured mold of the present invention, the gas source for performing the oxygen-containing plasma pretreatment in step (a) and generating the oxygen-containing plasma in step (b1) is selected from a group consisting of the following gases: 2 , O 3 , H 2 O, and any combination of the foregoing gases.
[0022] The method for making an anti-adhesive film on a nanostructured mold of the present invention further comprises a step (c) after the step (b), wherein the step (c) is to repeat the step (b) n times, where n is between 1 and 50.
[0023] In the method for making an anti-adhesive film on a nanostructured mold of the present invention, the output power of the oxygen-containing plasma pre-treatment in step (a) is between 10W and 450W, and the implementation time of step (a) is between 50 seconds and 6000 seconds.
[0024] In the method for making an anti-adhesive film on a nanostructured mold of the present invention, the process temperature in step (b) is between 10° C. and 100° C.
[0025] The beneficial effects of the present invention are as follows: based on the fact that the sub-step (b1) of the step (b) is implemented earlier than the sub-step (b3), and the precursor introduced in the sub-step (b3) is a carbon-silicon long-chain compound with a carbon number between 3 and 20, on the one hand, each dangling bond formed on the surface of the nanostructure by the oxygen-containing plasma of the sub-step (b1) can be equivalent to a highly active reaction point of the sub-step (b3), resulting in the dangling bond formed on the surface of the nanostructure by the sub-step (b1) to increase the reaction activity of the precursor of the sub-step (b3); on the other hand, the dangling bond energy increases, so that the carbon-silicon long-chain compound introduced in the sub-step (b3) not only increases the probability of reacting to generate the anti-adhesive film, but also helps to improve the adhesion of the generated anti-adhesive film to the surface of the nanostructure. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Other features and effects of the present invention will be clearly presented in the embodiments with reference to the accompanying drawings, in which:
[0027] Figure 1 is a schematic diagram of a production process, illustrating an existing NIL;
[0028] Figure 2 is a scanning electron microscope (SEM) cross-sectional image, illustrating that a specific example 1 (E1) of an anti-adhesive film produced by the method of the present invention for producing an anti-adhesive film on a mold having a nanostructure has a uniform thickness;
[0029] Figure 3 is a tensile test curve diagram illustrating the tensile test result of the anti-adhesive film of the specific example 1 (E1) of the present invention;
[0030] Figure 4a and Figure 4b is a SEM cross-sectional image, illustrating a specific example 2 (E2) of an anti-sticking film produced by the method of the present invention for producing an anti-sticking film on a mold having a nanostructure;
[0031] Figure 5 yes Figure 4a A partial magnified transmission electron microscope (TEM) cross-sectional image of , illustrating that the anti-adhesive film of the specific example 2 (E2) of the present invention has a uniform thickness; and
[0032] Figure 6 It is a tensile test curve diagram illustrating the tensile test result of the anti-adhesive film of the specific example 2 (E2) of the present invention. DETAILED DESCRIPTION
[0033] An embodiment of the method for making an anti-adhesive film on a mold having a nanostructure according to the present invention comprises the following steps: a step (a), a step (b), and a step (c).
[0034] The step (a) is to apply an oxygen-containing plasma pre-treatment to a mold, the surface of which has a nanostructure. Preferably, an output power of the oxygen-containing plasma pre-treatment of the step (a) is between 10W and 450W, and an implementation time of the step (a) is between 50 seconds and 6000 seconds; the nanostructure of the mold is made of a polymer, metal, semiconductor, ceramic, or glass material; the nanostructure of the mold is selected from nanopores, nanopillars, or nanotrenches, and the aspect ratios of the nanopores, nanopillars, and nanotrenches are all between 1.7 and 10. More preferably, an output power of the oxygen-containing plasma pre-treatment of the step (a) is between 30W and 450W, and an implementation time of the step (a) is between 120 seconds and 6000 seconds; the sizes of the nanopores, nanopillars, and nanotrenches are all between 50nm and 400nm.
[0035] The step (b) is to deposit an anti-adhesive film on the surface of the nanostructure by PEALD in a reaction chamber provided with the mold after the step (a). The step (b) has the following sub-steps in sequence: a first step (b1), a first step (b2), a first step (b3), and a first step (b4).
[0036] The step (b1) is to introduce an oxygen-containing plasma into the reaction chamber and immerse the mold in the oxygen-containing plasma to form a plurality of dangling bonds on the surface of the nanostructure.
[0037] Preferably, a gas source for performing the oxygen-containing plasma pre-treatment of step (a) and generating the oxygen-containing plasma of step (b1) is selected from a group consisting of: 2 , O 3 , H 2 O, and any combination of the foregoing gases.
[0038] The sub-step (b2) is to clear the oxygen-containing plasma in the reaction chamber.
[0039] The step (b3) is to introduce a precursor into the reaction chamber and immerse the mold in the precursor to react with the dangling bonds on the surface of the nanostructure and produce a by-product, thereby forming the anti-adhesive film on the surface of the nanostructure.
[0040] The precursor suitable for this embodiment of the present invention is a carbon-silicon long-chain compound with a carbon number between 3 and 20. For example, dichlorodimethylsilane (DDMS) and n-octadecyltrichlorosilane (ODTS). Preferably, the carbon chain of the carbon-silicon long-chain compound carries a halogen, and the silicon group carries a functional group capable of undergoing a hydrolysis condensation reaction; for example, an alkoxy group. For example, the carbon-silicon long-chain compound is selected from 1H,1H,2H,2H-perfluorooctyltriethoxysilane (FOTS), or 1H,1H,2H,2H-perfluorodecyltrichlorosilane (FDTS).
[0041] The sub-step (b4) is to remove by-products in the reaction chamber.
[0042] The step (c) is to repeat the step (b) n times, and one time of performing the step (b) is called one cycle. Preferably, n is between 1 and 50.
[0043] It should be added here that the main purpose of implementing the sub-step (b1) of each step (b) of the embodiment of the present invention earlier than the corresponding sub-step (b3) is that each dangling bond formed by the oxygen-containing plasma of each sub-step (b1) on the surface of the nanostructure is equivalent to a reaction point of the corresponding sub-step (b3). Therefore, the dangling bond formed on the surface of the nanostructure by each sub-step (b1) can increase the reaction point of the precursor (carbon-silicon long-chain compound) of the corresponding sub-step (b3). Taking the first cycle as an example, it is not only conducive to the formation of the anti-adhesive film of the first cycle, but also conducive to improving the adhesion of the anti-adhesive film generated in the first cycle to the surface of the nanostructure.
[0044] Preferably, the process temperature in step (b) is between 10°C and 100°C.
[0045] The present invention provides several specific examples and their corresponding test results based on this embodiment, which are described in detail as follows.
[0046] <Concrete example 1 (E1)>
[0047] In a specific example 1 (E1) of the method for making an anti-adhesive film on a mold having a nanostructure of the present invention, a mold having a nanostructure made of a photoresist (hereinafter referred to as PR) is first placed in a vacuum reaction chamber, and a plasma output power of 30 W and a duration of 120 seconds are applied to a surface of the nanostructure of the mold in the reaction chamber. 2 Plasma pre-treatment In the specific example 1 (E1) of the present invention, the mold is made of polycarbonate (hereinafter referred to as PC).
[0048] Then, 50 cycles of PEALD were performed at a process temperature of 70° C. Specifically, each cycle of PEALD was performed by sequentially introducing O 2 Plasma, immerse the mold in O 2 The reaction chamber was heated in a plasma for 20 seconds to form a plurality of dangling bonds on the surface of the nanostructure; an argon gas (Ar) was introduced into the reaction chamber for 10 seconds to remove the O 2 Plasma; introducing FOTS into the reaction chamber so that the mold is immersed in FOTS for 20 seconds to react with the dangling bonds on the surface of the nanostructure and produce a by-product, thereby generating a FOTS anti-adhesive film on the surface of the nanostructure for each cycle; introducing Ar into the reaction chamber for 10 seconds to remove the by-products in the reaction chamber.
[0049] The present invention also generates a FOTS anti-adhesive film on a PR layer on a PC plate under the same process conditions as the specific example 1 (E1) as a first evaluation test piece for evaluating the water contact angle; wherein a surface of the PR layer of the first evaluation test piece does not have a nanostructure. In addition, a second evaluation test piece is provided on which a PR layer without a nanostructure is formed on a PC plate; wherein the FOTS anti-adhesive film of the specific example 1 (E1) of the present invention is not generated on the PR layer of the second evaluation test piece. From the test results of the water contact angle (not shown), it can be obtained that the water contact angle of the second evaluation test piece is only 41 degrees, while the water contact angle of the first evaluation test piece has been increased to 92 degrees. It is preliminarily speculated that the anti-adhesive film generated by the specific example 1 (E1) of the present invention should have anti-adhesive properties.
[0050] <Concrete example 2 (E2)>
[0051] A specific example 2 (E2) of the method for making an anti-adhesive film on a mold having a nanostructure of the present invention is substantially the same as the specific example 1 (E1), except that a nanostructure of the specific example 2 (E2) is different from that of the specific example 1 (E1), and the nanostructure of ... 2The plasma pretreatment was performed with a plasma output power of 300 W and a duration of 600 seconds. PEALD was performed for 20 cycles at a process temperature of 25° C. In detail, each cycle of PEALD in Example 2 (E2) of the present invention was performed by sequentially introducing H with a plasma output power of 150 W into the reaction chamber. 2 O plasma, immerse the mold in H 2 O plasma for 15 seconds to form a plurality of dangling bonds on the surface of the nanostructure; Argon (Ar) is introduced into the reaction chamber for 10 seconds to remove H 2 O plasma; FOTS is introduced into the reaction chamber so that the mold is immersed in FOTS for 10 seconds to react with the dangling bonds on the surface of the nanostructure and produce a by-product, thereby generating a FOTS film of each cycle on the surface of the nanostructure; Ar is introduced into the reaction chamber for 10 seconds to remove the by-products in the reaction chamber. The present invention also generates a FOTS anti-adhesive film on a PR layer on a PC plate under the same process conditions as the specific example 2 (E2) as a third evaluation test piece for evaluating the water contact angle; wherein a surface of the PR layer of the third evaluation test piece does not have a nanostructure. In addition, a fourth evaluation test piece is also provided on which a PR layer without a nanostructure is formed on a PC plate; wherein the FOTS anti-adhesive film of the specific example 2 (E2) of the present invention is not generated on the PR layer of the fourth evaluation test piece. From the test results of the water contact angle (not shown), it can be seen that the water contact angle of the fourth evaluation test piece is only 39 degrees, while the water contact angle of the third evaluation test piece has been increased to 116 degrees. It can also be preliminarily inferred that the FOTS anti-adhesive film produced in the specific example 2 (E2) of the present invention should have better anti-adhesive properties.
[0052] It should be noted here that, in order to prove that the FOTS anti-adhesive film produced by the process conditions of the specific examples (E1 and E2) of the present invention has excellent anti-adhesive properties, the present invention also produces a FOTS anti-adhesive film on a steel plate for a tensile test according to the specification code ASTM-D3330A-04 (2018) using the process conditions of the specific examples (E1 and E2). The tensile test of the specific examples (E1 and E2) will be described later.
[0053] Depend on Figure 2 From the displayed SEM cross-sectional image, it can be seen that the PR nanostructure on the PC mold of the specific example 1 (E1) of the present invention is a nano-groove, the width and depth of which are 100nm and 250nm respectively (the calculated aspect ratio is 2.5), the distance between adjacent nano-grooves is 500nm, and the thickness of the FOTS anti-adhesive film generated by 50 cycles of PEALD is between 31.7nm and 33.7nm, and the thickness is quite uniform.
[0054] Then by Figure 3From the tensile test curve shown, it can be seen that the tensile test curve (blank curve) of the steel plate without the FOTS anti-adhesive film of the specific example 1 (E1) of the present invention is as high as 800gf to 850gf. On the contrary, the tensile curve of the FOTS anti-adhesive film of the specific example 1 (E1) of the present invention after 10 consecutive tensile tests shows that the first, fifth and tenth tensile test curves are between 500gf and 650gf. Although the tensile value increases slowly, it is still more than 30% lower than the blank curve. It is confirmed that the FOTS anti-adhesive film generated by the method of the specific example 1 (E1) of the present invention has excellent anti-adhesive properties. In addition, the PR nano-grooves on the PC mold of the specific example 1 (E1) of the present invention are further transferred to a PR layer on a glass substrate, and the number of transfers can reach 11 to 12 times or more.
[0055] Depend on Figure 4a , Figure 4b and Figure 5 The SEM and TEM cross-sectional images respectively show that the PR nanostructure on the PC mold of the specific example 2 (E2) of the present invention is a sawtooth nanocolumn with a narrow top and a wide bottom. The bottom width, half-height width and height of the sawtooth nanocolumn are about 200nm, 86nm and 365nm respectively (the calculated aspect ratio is between 1.83 and 4.24), and the FOTS anti-adhesive film ( Figure 5 The thickness at the mark A is between 3.5 nm and 3.0 nm, and the thickness is quite uniform.
[0056] Then by Figure 6 From the tensile test curve shown, it can be seen that the tensile test curve (blank curve) of the steel plate without the FOTS anti-adhesive film of the specific example 2 (E2) of the present invention is as high as 800gf to 950gf. On the contrary, the tensile curve of the FOTS anti-adhesive film of the specific example 2 (E2) of the present invention after 10 consecutive tensile tests shows that the first, fifth and tenth tensile test curves are only between 400gf and 600gf, which is not only reduced by more than 50% relative to the blank curve, but also has no upward trend in the tensile value after 10 consecutive tensile tests. It also proves that the FOTS anti-adhesive film generated by the method of the specific example 2 (E2) of the present invention has excellent anti-adhesive properties. Furthermore, the PR sawtooth nanocolumns on the PC mold of the specific example 2 (E2) of the present invention are further transferred to a PR layer on a glass substrate, and the number of transfers can exceed 30 times, effectively improving the service life of the mold.
[0057] As can be seen from the above detailed description of the present invention, the present invention is based on the implementation of the sub-step (b1) of each step (b) earlier than the corresponding sub-step (b3), so that each dangling bond formed by the oxygen-containing plasma of each sub-step (b1) on the surface of the nanostructure is equivalent to a reaction point of the corresponding sub-step (b3), resulting in the dangling bond formed on the surface of the nanostructure in each sub-step (b1) to increase the reaction point of the precursor (carbon-silicon long-chain compound) of the corresponding sub-step (b3). In addition, the precursor selected by the present invention is a carbon-silicon long-chain compound with a carbon number between 3 and 20, whose carbon chain has a halogen (such as fluorine), and the silicon base has a functional group that can undergo a hydrolysis-condensation reaction. Therefore, for the first cycle of PEALD, the increase of dangling bonds is not only beneficial for the carbon-silicon long-chain compound to undergo a hydrolysis-condensation reaction in the first cycle to generate its anti-adhesive film, but also beneficial for improving the adhesion of the anti-adhesive film generated in the first cycle to the surface of the nanostructure.
[0058] In summary, the method of the present invention for making an anti-adhesive film on a mold having a nanostructure can not only increase the hydrolysis condensation reaction activity of the carbon-silicon long-chain compound in the first cycle to generate its anti-adhesive film, but also help to improve the adhesion between the anti-adhesive film generated in the first cycle and the surface of the nanostructure, thereby increasing the service life of the mold, so the purpose of the present invention can be achieved.
[0059] However, what is described above is only an embodiment of the present invention and should not be used to limit the scope of implementation of the present invention. All simple equivalent changes and modifications made according to the claims and description of the present invention are still within the scope of the present invention.
Claims
1. A method for making an anti-adhesive film on a mold having a nanostructure, characterized in that: It includes the following steps: Step (a), subjecting the mold to oxygen-containing plasma pre-treatment, wherein the surface of the mold has a nanostructure; and Step (b), after step (a), depositing an anti-adhesive film on the surface of the nanostructure by plasma-assisted atomic layer deposition in a reaction chamber provided with the mold, step (b) sequentially comprises the following sub-steps: In the next step (b1), oxygen-containing plasma is introduced into the reaction chamber, and the mold is immersed in the oxygen-containing plasma to form a plurality of dangling bonds on the surface of the nanostructure. In the next step (b2), the oxygen-containing plasma in the reaction chamber is removed. In the next step (b3), a precursor is introduced into the reaction chamber, and the mold is immersed in the precursor to react with the dangling bonds on the surface of the nanostructure and produce by-products, thereby forming the anti-adhesive film on the surface of the nanostructure, and The next step (b4) is to remove the by-products in the reaction chamber; The precursor is a carbon-silicon long-chain compound with a carbon number between 3 and 20.
2. The method for producing an anti-adhesive film on a mold having a nanostructure according to claim 1, characterized in that: The carbon chain of the carbon-silicon long-chain compound carries halogen, and the silicon base carries a functional group capable of undergoing hydrolysis and condensation reactions.
3. The method for preparing an anti-adhesive film on a mold having a nanostructure according to claim 1, characterized in that: The carbon-silicon long-chain compound is selected from 1H, 1H, 2H, 2H-perfluorooctyltriethoxysilane, 1H, 1H, 2H, 2H-perfluorodecyltrichlorosilane, octadecyltrichlorosilane, or dimethyldichlorosilane.
4. The method for producing an anti-adhesive film on a mold having a nanostructure according to claim 1, characterized in that: The nanostructure of the mold is made of a material selected from polymer, metal, semiconductor, ceramic, or glass.
5. The method for producing an anti-adhesive film on a mold having a nanostructure according to claim 1, characterized in that: The nanostructure of the mold is selected from nanoholes, nanocolumns or nanogrooves, and the aspect ratios of the nanoholes, nanocolumns and nanogrooves are all between 1.7 and 10.
6. The method for producing an anti-adhesive film on a mold having a nanostructure according to claim 5, characterized in that: The sizes of the nanopores, nanopillars and nanotrench are all between 50nm and 400nm.
7. The method for producing an anti-adhesive film on a mold having a nanostructure according to claim 1, characterized in that: The gas source for performing the oxygen-containing plasma pre-treatment of step (a) and generating the oxygen-containing plasma of step (b1) is selected from a group consisting of: O2, O3, H2O, and any combination of the aforementioned gases.
8. The method for producing an anti-adhesive film on a mold having a nanostructure according to claim 7, characterized in that: The method further comprises a step (c) after the step (b), wherein the step (c) is to repeat the step (b) n times, where n is between 1 and 50.
9. The method for producing an anti-adhesive film on a mold having a nanostructure according to claim 8, characterized in that: The output power of the oxygen-containing plasma pre-treatment in step (a) is between 10W and 450W, and the implementation time of step (a) is between 50 seconds and 6000 seconds.
10. The method for producing an anti-adhesive film on a mold having a nanostructure according to claim 1, characterized in that: The process temperature in step (b) is between 10°C and 100°C.