Water electrolysis positive electrode catalyst as well as preparation method and application thereof
The method of preparing a cathode catalyst using nano oxide carriers and ruthenium chloride addresses the corrosion and resistance issues of existing catalysts, resulting in efficient and durable water electrolysis performance.
Patent Information
- Application Number
- CN202411173499.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
Existing water electrolysis technologies face challenges with catalysts like IrO2 and RuO2 corroding in acidic environments, leading to decreased efficiency and high electrical resistance, and other methods are either complex or not suitable for proton exchange membrane (PEM) water electrolyzers.
A method involving ultrasonic dispersion of nano oxide carriers in water, hydrothermal reduction of ruthenium chloride, and application of the resulting catalyst on a proton exchange membrane with Nafion solution to create a stable and efficient cathode catalyst.
The catalysts resist acid corrosion and reduce resistance, achieving a voltage of 1.5-1.72V with high catalytic performance and extended service life.
Smart Images

Figure CN119061412A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of PEM water electrolysis, and specifically relates to a water electrolysis positive electrode catalyst and a preparation method and application thereof. Background Art
[0002] As the global demand for clean energy continues to grow, the development and application of hydrogen as a pollution-free and efficient energy carrier has attracted widespread attention. As an effective way to obtain hydrogen, the technological development of water electrolysis is of great significance for solving environmental crises and energy shortages. However, the existing water electrolysis technology still faces some technical challenges in practical applications.
[0003] In proton exchange membrane (PEM) water electrolyzers, the acidic environment places higher demands on the selection and stability of catalysts. Currently, although commonly used oxide catalysts such as IrO2 and RuO2 have certain catalytic activity, they are susceptible to corrosion under acidic conditions, resulting in decreased electrolysis efficiency. In addition, the electrical resistance of these oxides is relatively high, further increasing the energy consumption during the electrolysis process.
[0004] Patent 202311262834.5 discloses a silicon oxide supported iridium catalyst and its preparation method and application. When the mass of iridium nanoparticles accounts for 30wt% of the total mass of the catalyst, the 2 In the case of , the overpotential reaches 310mV, and high iridium loading is still required to achieve higher electrolyzer performance. Patent 202311151658.8 proposes a PdRu / MOx / NF composite material, a preparation method and application thereof. Although this method shows certain advantages in the alkaline electrolysis of water, its preparation process is complicated and is not suitable for PEM water electrolyzers in acidic environments, which limits its practicality in a wider range of application scenarios. Patent CN111060560A proposes a Ru-WO3 nanomaterial, a preparation method and application thereof, specifically, Ru nanoparticles are uniformly loaded on the surface of WO3 nanoparticles to obtain flaky crystals with a length of 150-160nm, a width of 150-160nm and a thickness of 25-30nm. The patent uses ethylene glycol to reduce ruthenium chloride, and the reaction is slow and the reduction is incomplete. Patent CN111715239A proposes a method for preparing oxide-supported single-atom catalysts, claiming that single-atom catalysts of Al, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Mo, Ru, Rh, Ag, Cd, In, Sn, W, Re, Ir, Pt, Au, Bi, and Er are prepared. In practice, only Ir, Pt, Pd, and Au catalysts are prepared. Since the photos provided are not original TEM electron microscope photos, they lack persuasiveness. Moreover, the thermodynamics of preparing metallic Al single atoms by carbonization method is not feasible. Summary of the invention
[0005] In view of the above problems existing in the prior art, the present application provides a water electrolysis cathode catalyst and a preparation method and application thereof.
[0006] To solve the above problems, the present invention provides the following technical solutions:
[0007] In a first aspect, the present application provides a method for preparing a positive electrode catalyst for water electrolysis, comprising the following steps:
[0008] S1, ultrasonically dispersing the nano oxide carrier in deionized water to prepare a dispersion;
[0009] S2. Dissolve ruthenium chloride in hydrochloric acid solution, add it to the dispersion while stirring, add reducing agent dropwise, keep warm in an autoclave for hydrothermal reduction reaction, filter, wash and dry after the reaction is completed, and obtain a catalyst; take out the catalyst, crush it, mix it with Nafion solution, and apply it on a proton exchange membrane as a positive electrode catalyst for water electrolysis.
[0010] In one embodiment of the present application, in step S1, the nano oxide carrier is selected from one of tungsten oxide, molybdenum oxide, titanium oxide, tin oxide, germanium oxide, and tantalum oxide.
[0011] In one embodiment of the present application, in step S1, the usage ratio of nano-oxide to deionized water is 1 mg:10 mL.
[0012] In one embodiment of the present application, in step S2, the concentration of the hydrochloric acid solution is 0.1 mol / L-6 mol / L.
[0013] In one embodiment of the present application, the usage ratio of ruthenium chloride to hydrochloric acid solution is 1 mg:50 mL.
[0014] In one embodiment of the present application, in step S2, the reducing agent is selected from one of hydrazine, formaldehyde, glycerol, and ethanol.
[0015] In one embodiment of the present application, in step S2, according to the stoichiometric ratio, the amount of the reducing agent used is 1-4 times the stoichiometric ratio.
[0016] In one embodiment of the present application, in step S2, according to the stoichiometric ratio, the amount of the reducing agent used is 1-2 times the stoichiometric ratio.
[0017] In one embodiment of the present application, in step S2, the temperature of the hydrothermal reduction reaction is 80-140° C.; the time of the hydrothermal reduction reaction is 2-8 hours.
[0018] In one embodiment of the present application, in step S2, the drying temperature is 80° C. and the drying time is 6 hours.
[0019] In one embodiment of the present application, in step S2, the loading amount of ruthenium particles in the catalyst is 10 wt.%; and the particle size of the ruthenium particles in the catalyst is 4-10 nm.
[0020] In one embodiment of the present application, in step S2, the mass fraction of the Nafion solution is 5wt.%,
[0021] In one embodiment of the present application, in step S2, the usage ratio of the catalyst to the Nafion solution is 1 mg:2 mL.
[0022] In one embodiment of the present application, the coating amount of the positive electrode catalyst on the proton exchange membrane is 0.4 mg / cm 2 .
[0023] In a second aspect, the present application provides a positive electrode catalyst for water electrolysis prepared using the above method.
[0024] In a third aspect, the present application provides the use of a water electrolysis cathode catalyst in PEM water electrolysis to produce hydrogen.
[0025] Compared with the prior art, the present invention loads Ru inert metal on nano oxide carrier as positive electrode catalyst for water electrolysis. Ru inert metal can resist acid corrosion and reduce resistance at the same time. 2 The voltage under the condition is 1.5-1.72V, and the catalyst has high catalytic performance and service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The Ru / WO3 catalyst was used as the positive electrode, with a Ru loading of 0.4 mg / cm 2 , the negative electrode is platinum black catalyst with a loading of 0.4 mg / cm 2 Performance curve of water electrolyzer. DETAILED DESCRIPTION
[0027] The following will provide a clear and complete description of the technical solutions in the embodiments of the present application in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.
[0028] The "range" disclosed in this application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range.
[0029] Unless otherwise specified, when the present invention relates to the percentage between liquids, the percentage is volume / volume percentage; when the present invention relates to the percentage between liquids and solids, the percentage is volume / weight percentage; when the present invention relates to the percentage between solids and liquids, the percentage is weight / volume percentage; the rest are weight / weight percentages.
[0030] Example 1
[0031] 30 mg of WO3 with a diameter of 200 nm was placed in 300 mL of deionized water and dispersed by ultrasound. 0.4 mg of ruthenium chloride was dissolved in 20 mL of 6 mol / L hydrochloric acid solution, poured into the above deionized water while stirring, and a 1:20 diluted hydrazine solution was added dropwise, and the stoichiometric ratio of the reducing agent was added according to the stoichiometric ratio of 1:1. The above solution was placed in an autoclave and kept warm at 80°C for 2 hours. After the reaction was completed and cooled, the solution was taken out for filtration and washing, and the obtained solid phase catalyst was dried in a vacuum drying oven at 80°C for 6 hours. The catalyst was taken out and crushed to obtain a catalyst with ruthenium particles with a diameter of 10 nm. 5 mL of Nafion solution was mixed (the mass fraction of Nafion solution was 5 wt.%, and the solvent was methanol), the amount ratio of catalyst to 5 wt.% Nafion solution was 1 mg:2 mL, and 10 times the mass of isopropanol was added, and after mixing, it was coated on the proton exchange membrane 212 membrane as a positive electrode catalyst, and the coating amount was 0.4 mg / cm 2 Metal catalyst, platinum black is used as the negative electrode catalyst. Then MEA is made to test its water electrolysis performance. The measured water electrolysis current density is 1A / cm 2 The voltage of the case is 1.6V.
[0032] Example 2
[0033] 30 mg of MoO3 with a diameter of 200 nm was placed in 300 mL of deionized water and dispersed by ultrasound. 0.4 mg of ruthenium chloride was dissolved in 20 mL of 0.1 mol / L hydrochloric acid solution, poured into the above deionized water while stirring, and a 1:20 diluted formaldehyde solution was added dropwise, and the reducing agent was added according to the stoichiometric ratio of 2:1. The above solution was placed in an autoclave and kept warm at 80 ° C for 4 hours. After the reaction was completed and cooled, the solution was taken out for filtration and washing, and the obtained solid phase catalyst was dried in a vacuum drying oven at 80 ° C for 6 hours. The catalyst was taken out and crushed to obtain a catalyst with a diameter of 5 nm ruthenium particles, and the loading was maintained at 1:10. Take 5mL of Nafion solution (the mass fraction of Nafion solution is 5wt.%, and the solvent is methanol), the amount ratio of catalyst to 5wt.% Nafion solution is 1mg:2mL, and then add 10 times the mass of isopropanol, and then coat the mixture on the proton exchange membrane 212 as the positive electrode catalyst, and the coating amount is 0.4mg / cm 2 Metal catalyst, platinum black is used as the negative electrode catalyst. Then MEA is made to test its water electrolysis performance. The measured water electrolysis current density is 1A / cm 2 The voltage of the case is 1.5V.
[0034] Example 3
[0035] 30 mg of TiO2 with a diameter of 200 nm was placed in 300 mL of deionized water and dispersed by ultrasound. 0.4 mg of ruthenium chloride was dissolved in 20 mL of 0.1 mol / L hydrochloric acid solution, poured into the above deionized water while stirring, and a 1:20 diluted propylene glycol solution was added dropwise, and the reducing agent was added according to the stoichiometric ratio of 3:1. The above solution was placed in an autoclave and kept at 100 ° C for 4 hours. After the reaction was completed and cooled, the solution was taken out for filtration and washing, and the obtained solid phase catalyst was dried in a vacuum drying oven at 80 ° C for 6 hours. The catalyst was taken out and crushed to obtain a catalyst with a diameter of 6 nm ruthenium particles, and the loading was maintained at 1:10. Take 5mL of Nafion solution (the mass fraction of Nafion solution is 5wt.%, and the solvent is methanol), the amount ratio of catalyst to 5wt.% Nafion solution is 1mg:2mL, and then add 10 times the mass of isopropanol, and then coat the mixture on the proton exchange membrane 212 as the positive electrode catalyst, and the coating amount is 0.4mg / cm 2 Metal catalyst, platinum black is used as the negative electrode catalyst. Then MEA is made to test its water electrolysis performance. The measured water electrolysis current density is 1A / cm 2 The voltage in the case is 1.72V.
[0036] Example 4
[0037] 30 mg of SnO2 with a diameter of 200 nm was placed in 300 mL of deionized water and dispersed by ultrasound. 0.4 mg of ruthenium chloride was dissolved in 20 mL of 0.1 mol / L hydrochloric acid solution, poured into the above deionized water while stirring, and a 1:20 diluted propylene glycol solution was added dropwise, and the reducing agent was added according to the stoichiometric ratio of 3:1. The above solution was placed in an autoclave and kept warm at 120 ° C for 5 h. After the reaction was completed and cooled, the solution was taken out for filtration and washing, and the obtained solid phase catalyst was dried in a vacuum drying oven at 80 ° C for 6 h. The catalyst was taken out and crushed to obtain a catalyst with a diameter of 4.5 nm ruthenium particles, and the loading was maintained at 1:10. Take 5mL of Nafion solution (the mass fraction of Nafion solution is 5wt.%, and the solvent is methanol), the amount ratio of catalyst to 5wt.% Nafion solution is 1mg:2mL, and then add 10 times the mass of isopropanol, and then coat the mixture on the proton exchange membrane 212 as the positive electrode catalyst, and the coating amount is 0.4mg / cm 2 Metal catalyst, platinum black is used as the negative electrode catalyst. Then MEA is made to test its water electrolysis performance. The measured water electrolysis current density is 1A / cm 2 The voltage of the case is 1.58V.
[0038] Example 5
[0039] 30 mg of GeO2 with a diameter of 200 nm was placed in 300 mL of deionized water and dispersed by ultrasound. 0.4 mg of ruthenium chloride was dissolved in 20 mL of 0.1 mol / L hydrochloric acid solution, poured into the above deionized water while stirring, and a 1:20 diluted propylene glycol solution was added dropwise, and the reducing agent was added according to the stoichiometric ratio of 4:1. The above solution was placed in an autoclave and kept at 140 ° C for 3 h. After the reaction was completed and cooled, the solution was taken out for filtration and washing, and the obtained solid phase catalyst was dried in a vacuum drying oven at 80 ° C for 6 h. The catalyst was taken out and crushed to obtain a catalyst with a diameter of 4 nm ruthenium particles, and the loading was maintained at 1:10. Take 5mL of Nafion solution (the mass fraction of Nafion solution is 5wt.%, and the solvent is methanol), the amount ratio of catalyst to 5wt.% Nafion solution is 1mg:2mL, and then add 10 times the mass of isopropanol, and then coat the mixture on the proton exchange membrane 212 as the positive electrode catalyst, and the coating amount is 0.4mg / cm 2 Metal catalyst, platinum black is used as the negative electrode catalyst. Then MEA is made to test its water electrolysis performance. The measured water electrolysis current density is 1A / cm 2 The voltage in the case is 1.53V.
[0040] Example 6
[0041] 30 mg of Ta2O5 with a diameter of 200 nm was placed in 300 mL of deionized water and dispersed by ultrasound. 0.4 mg of ruthenium chloride was dissolved in 20 mL of 0.1 mol / L hydrochloric acid solution, poured into the above deionized water while stirring, and a 1:20 diluted propylene glycol solution was added dropwise, and the reducing agent was added according to the stoichiometric ratio of 4:1. The above solution was placed in an autoclave and kept warm at 140°C for 3 hours. After the reaction was completed and cooled, the solution was taken out for filtration and washing, and the obtained solid phase catalyst was dried in a vacuum drying oven at 80°C for 6 hours. The catalyst was taken out and crushed to obtain a catalyst with a diameter of 4 nm ruthenium particles, and the loading was maintained at 1:10. Take 5mL of Nafion solution (the mass fraction of Nafion solution is 5wt.%, and the solvent is methanol), the amount ratio of catalyst to 5wt.% Nafion solution is 1mg:2mL, and then add 10 times the mass of isopropanol, and then coat the mixture on the proton exchange membrane 212 as the positive electrode catalyst, and the coating amount is 0.4mg / cm 2 Metal catalyst, platinum black is used as the negative electrode catalyst. Then MEA is made to test its water electrolysis performance. The measured water electrolysis current density is 1A / cm 2 The voltage in the case is 1.59V.
[0042] The present application is described in detail above in conjunction with specific implementation methods and exemplary embodiments, but these descriptions cannot be understood as limiting the present application. Those skilled in the art understand that, without departing from the spirit and scope of the present application, the technical solution of the present application and its implementation methods may be subjected to a variety of equivalent substitutions, modifications or improvements, all of which fall within the scope of the present application.
Claims
1. A method for preparing a positive electrode catalyst for water electrolysis, characterized in that: The following steps are involved: S1, ultrasonically dispersing the nano oxide carrier in deionized water to prepare a dispersion; S2. Dissolve ruthenium chloride in hydrochloric acid solution, add it to the dispersion while stirring, add reducing agent dropwise, keep warm in an autoclave for hydrothermal reduction reaction, filter, wash and dry after the reaction is completed, and obtain a catalyst; take out the catalyst, crush it, mix it with Nafion solution, and apply it on a proton exchange membrane as a positive electrode catalyst for water electrolysis.
2. The method for preparing a positive electrode catalyst for water electrolysis according to claim 1, characterized in that: In step S1, the nano oxide carrier is selected from one of tungsten oxide, molybdenum oxide, titanium oxide, tin oxide, germanium oxide and tantalum oxide.
3. The method for preparing a positive electrode catalyst for water electrolysis according to claim 1, characterized in that: In step S1, the dosage ratio of the nano-oxide to deionized water is 1 mg:10 mL.
4. The method for preparing a positive electrode catalyst for water electrolysis according to claim 1, characterized in that: In step S2, the concentration of the hydrochloric acid solution is 0.1 mol / L-6 mol / L; the dosage ratio of the ruthenium chloride to the hydrochloric acid solution is 1 mg:50 mL.
5. The method for preparing a positive electrode catalyst for water electrolysis according to claim 1, characterized in that: In step S2, the reducing agent is selected from one of hydrazine, formaldehyde, glycerol and ethanol; according to the stoichiometric ratio, the amount of the reducing agent is 1-4 times the stoichiometric ratio.
6. The method for preparing a positive electrode catalyst for water electrolysis according to claim 1, characterized in that: In step S2, the temperature of the hydrothermal reduction reaction is 80-140° C.; the time of the hydrothermal reduction reaction is 2-8 hours.
7. The method for preparing a positive electrode catalyst for water electrolysis according to claim 1, characterized in that: In step S2, the loading amount of ruthenium particles in the catalyst is 10wt.%; the particle size of the ruthenium particles in the catalyst is 4-10nm.
8. The method for preparing a positive electrode catalyst for water electrolysis according to claim 1, characterized in that: In step S2, the mass fraction of Nafion solution is 5wt.%; the amount ratio of catalyst to Nafion solution is 1mg:2mL; the coating amount of positive electrode catalyst on the proton exchange membrane is 0.4mg / cm 2 .
9. A positive electrode catalyst for water electrolysis prepared by the method according to any one of claims 1 to 8.
10. Use of the water electrolysis cathode catalyst according to claim 9 in PEM water electrolysis to produce hydrogen.