PEM electrolytic bath pole plate and preparation method and application thereof

By adopting a combined coating structure of precious metal and non-precious metal layers on the PEM electrolytic cell plate, combined with glow cleaning and ion source technology, the problem of difficult control of coating thickness and poor corrosion resistance is solved, and high-efficiency and environmentally friendly extremes are achieved Plate preparation reduces the use of precious metals and production costs.

CN119061419AInactive Publication Date: 2024-12-03CEMT CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411488430.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The thickness of the coating layer of the existing PEM electrolytic cell plate is difficult to control, and there are problems of pinhole defects and poor corrosion resistance. The use of organic solvents and heavy metal ions in conventional electroplating is not environmentally friendly, resulting in poor coating binding.

Method used

Using a combined coating structure of precious metal layer and non-precious metal layer, non-precious metal and precious metal coating are treated with the anode surface and the cathode surface respectively to reduce the use of precious metals, and use glow cleaning and ion source technology to improve the coating during the preparation process. and corrosion resistance.

Benefits of technology

It has achieved a significant reduction in the use of precious metals while ensuring conductive properties, improved the binding force and corrosion resistance of the coating, avoided defects such as pinholes, and reduced the use of toxic solvents, and improved product quality and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061419A_ABST
    Figure CN119061419A_ABST
Patent Text Reader

Abstract

The invention provides a PEM electrolytic cell polar plate and a preparation method and application thereof.The PEM electrolytic cell polar plate comprises a substrate, a cathode face and an anode face, the cathode face and the anode face are arranged on the surfaces of the two sides of the substrate respectively, and the anode face comprises a precious metal layer and an anode face non-precious metal layer arranged between the substrate and the precious metal layer; and the cathode surface comprises at least one cathode surface non-noble metal layer. The cost of the polar plate is greatly reduced under the condition that the corrosion resistance and the electrical property of the polar plate are ensured, and meanwhile, the defects of pinholes, pits, cracks and the like caused by conventional electroplating can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PEM water electrolysis hydrogen production, and relates to a PEM electrolyzer polar plate and a preparation method and application thereof. Background Art

[0002] Hydrogen is a clean energy source, but it does not exist naturally. It is often obtained through the conversion and extraction of different substances. Hydrogen is mainly produced through fossil fuel reforming, coal-to-hydrogen, industrial by-product hydrogen, etc., and is further used in petroleum refining, fine chemical synthesis, automobile fuel and residents' daily life. However, the preparation of hydrogen is highly polluting, and a cleaner hydrogen energy source is needed in the future. The most suitable technology is water electrolysis to produce hydrogen. The raw material of PEM water electrolysis is pure water, which does not produce pollution and has high hydrogen production efficiency. It is one of the current popular routes for hydrogen production research.

[0003] PEM plates are one of the key components of electrolyzers. PEM plates are mostly made of titanium plates, stainless steel plates, etc., and the preparation processes of the plates are mostly stamping, etching, etc. PEM plates undertake the functions of conducting electricity, transmitting water-gas mixtures, and supporting. Its coating needs to withstand a certain corrosion potential, have good conductivity, and have a long service life.

[0004] CN114875464A discloses a method for preparing an anode bipolar plate for a PEM electrolytic cell, comprising: (1) cutting a stainless steel metal substrate, followed by surface degreasing and pickling, and then immersion corrosion processing to form micro-nano cavities on the substrate surface; (2) ultrasonically cleaning the substrate after the above treatment, electroplating Ni and Ni-Cr composite layers on the surface, and then attaching a slurry consisting of conductive carbon black and epoxy resin, followed by curing, carbonizing and alloying to form a gradient coating, and finally performing composite rolling and stamping, and cleaning to obtain the anode bipolar plate for the PEM electrolytic cell.

[0005] CN117026319A discloses a method for preparing a partitioned coating on the surface of a bipolar plate of a PEM electrolyzer, comprising the following steps: A) pre-cleaning the bipolar plate; B) shielding the ridge side and bottom surfaces of the bipolar plate flow channel area obtained in step A); C) electroplating the ridge area of ​​the bipolar plate flow channel area obtained in step B).

[0006] In the method described in the above scheme, the thickness of the coating is not easy to control and the electroplating solution contains organic solvents and heavy metal ions, which are not environmentally friendly. The resulting coating has poor adhesion and is prone to plating peeling. At the same time, there are many pinhole defects, resulting in poor corrosion resistance. Summary of the invention

[0007] The object of the present invention is to provide a PEM electrolytic cell plate and a preparation method and application thereof. The present invention can significantly reduce the cost of the plate while ensuring the corrosion resistance and electrical properties of the plate, and can also avoid defects such as pinholes, pitting, cracks, etc. caused by conventional electroplating.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a PEM electrolyzer plate, comprising a substrate and a cathode surface and an anode surface respectively arranged on both side surfaces of the substrate, the anode surface comprising a precious metal layer and an anode surface non-precious metal layer arranged between the substrate and the precious metal layer, and the cathode surface comprising at least one cathode surface non-precious metal layer.

[0010] The PEM electrolyzer plate of the present invention adopts precious metal + non-precious metal on the anode surface and non-precious metal coating on the cathode surface, which greatly reduces the use of precious metals. Adding non-precious metal coating between the precious metal coating and the substrate can also further reduce the use of precious metal materials. Under the premise of excellent conductive performance, the bonding force is stronger and the corrosion resistance is higher.

[0011] Preferably, the substrate includes any one of a stainless steel plate, a titanium plate, an aluminum plate, a copper plate or a nickel plate, or a combination of at least two of them.

[0012] Preferably, the noble metal layer includes any one of Au, Pt, Ta, Ru or Ir or a combination of at least two thereof, preferably Au and / or Pt.

[0013] Preferably, the anode surface non-noble metal layer includes a single substance layer and / or a compound layer.

[0014] Preferably, the single-element layer includes any one of Ti, Nb, Cr, W or Ni or a combination of at least two of them, preferably Ti and / or Cr.

[0015] Preferably, the compound layer comprises any one of TiN, TiCN, TiC, NbC or CrN or a combination of at least two thereof, preferably any one of TiN, TiCN or TiC or a combination of at least two thereof.

[0016] Preferably, the thickness of the noble metal layer is 10-200 nm, for example, 10 nm, 50 nm, 100 nm, 150 nm or 200 nm.

[0017] Preferably, the thickness of the non-precious metal layer on the anode surface is 100-800 nm, for example, 100 nm, 200 nm, 300 nm, 500 nm or 800 nm.

[0018] Preferably, the cathode surface comprises a first cathode surface non-noble metal layer and a second cathode surface non-noble metal layer which are stacked in sequence.

[0019] Preferably, the first cathode side non-noble metal layer and the second cathode side non-noble metal layer independently include any one of a single substance layer, a compound layer, an amorphous carbon layer or a conductive polymer layer, or a combination of at least two thereof.

[0020] Preferably, the single-element layer includes any one of Ti, Nb, Cr, W or C or a combination of at least two thereof, preferably Ti and / or Cr.

[0021] Preferably, the compound layer comprises any one of TiN, TiCN, TiC, NbC or CrN or a combination of at least two thereof, preferably any one of TiN, TiCN or TiC or a combination of at least two thereof.

[0022] Preferably, the thickness of the cathode surface non-noble metal layer is independently 100-800 nm, for example, 100 nm, 200 nm, 300 nm, 500 nm or 800 nm.

[0023] In a second aspect, the present invention provides a method for preparing a PEM electrolyzer plate as described in the first aspect, the preparation method comprising the following steps:

[0024] (1) Glow cleaning of the substrate;

[0025] (2) performing a non-precious metal coating treatment on the anode surface of the glow-cleaned substrate to obtain a non-precious metal layer on the anode surface, and performing a precious metal coating treatment on the surface of the non-precious metal layer on the anode surface to obtain a substrate provided with an anode surface;

[0026] (3) On the other side of the substrate provided with the anode surface, a cathode surface non-precious metal coating treatment is performed to obtain the PEM electrolytic cell electrode plate.

[0027] In the preparation process of the PEM electrolytic cell plate of the present invention, steps (1) and (2) can be repeated in advance to prepare two substrates with anode surfaces, and the two substrates are laminated on the side plated with the precious metal layer and then the cathode surface is plated with non-precious metal. This can improve the preparation efficiency. Alternatively, the cathode surface can be plated directly on the other side of the substrate.

[0028] Preferably, pretreatment is performed before the glow cleaning in step (1).

[0029] Preferably, the pretreatment includes ultrasonic degreasing - ultrasonic pre-cleaning - secondary cleaning - pure water cleaning - drying.

[0030] Preferably, the temperature of the ultrasonic degreasing is 40-90°C, for example, 40°C, 50°C, 60°C, 80°C or 90°C.

[0031] Preferably, the drying temperature is 60-160°C, for example, 60°C, 80°C, 100°C, 140°C or 160°C.

[0032] Preferably, the glow cleaning comprises cleaning the substrate in an inert atmosphere by means of negative glow discharge and an ion source.

[0033] Preferably, the bias voltage of the glow cleaning is 500-1500V, for example, 500V, 600V, 700V, 800V or 1000V.

[0034] Preferably, the pressure of the inert atmosphere is 0.5~80Pa, for example: 0.5 Pa, 5 Pa, 10 Pa, 40 Pa or 80Pa, etc., preferably 1~10Pa.

[0035] Preferably, the ion source comprises any one of an anode layer ion source, a Hall ion source, a Kaufman ion source or a plasma source, or a combination of at least two thereof.

[0036] Preferably, the ion beam energy of the ion source is 100-500 eV, for example, 100 eV, 200 eV, 300 eV, 400 eV or 500 eV.

[0037] Preferably, the power of the ion source is 2-3 kW, for example, 2 kW, 2.2 kW, 2.5 kW, 2.8 kW or 3 kW.

[0038] Preferably, the glow cleaning time is 5 to 40 minutes, for example, 5 minutes, 10 minutes, 15 minutes, 20 minutes or 40 minutes.

[0039] Preferably, the coating treatment device in step (2) comprises a single converter and / or a continuous tunnel furnace.

[0040] Preferably, the coating process includes any one of multi-arc ion plating, magnetron sputtering or evaporation plating, or a combination of at least two of them.

[0041] Preferably, the bias voltage of the non-precious metal coating treatment on the anode surface is 50-600V, for example, 50V, 100V, 200V, 300V or 600V, etc., preferably 100-400V.

[0042] Preferably, the current of the non-precious metal coating treatment on the anode surface is 20-120A, for example: 20A, 50A, 80A, 100A or 120A, etc., preferably 80-100A.

[0043] Preferably, the gas used for the non-precious metal coating treatment on the anode surface includes any one of Ar, N2, CH4, C2H2, TiCl4 or H2, or a combination of at least two of them.

[0044] Preferably, the gas flow rate of the non-precious metal coating treatment on the anode surface is 100-500 sccm, for example: 100 sccm, 200 sccm, 300 sccm, 400 sccm or 500 sccm, etc., preferably 100-200 sccm.

[0045] Preferably, the non-precious metal coating treatment time of the anode surface is 1 to 60 min, for example: 1 min, 5 min, 10 min, 30 min or 60 min, etc., preferably 5 to 30 min.

[0046] Preferably, the bias voltage of the precious metal coating treatment in step (2) is 100-600V, for example: 100V, 150V, 200V, 300V or 600V.

[0047] Preferably, the gas flow rate of the noble metal coating process is 50-600 sccm, for example, 50 sccm, 200 sccm, 300 sccm, 400 sccm or 600 sccm.

[0048] Preferably, the precious metal coating treatment time is 2 to 20 minutes, for example: 2 minutes, 5 minutes, 10 minutes, 15 minutes or 20 minutes, etc.

[0049] Preferably, the noble metal coating process is followed by a furnace cooling process.

[0050] Preferably, the atmosphere for the cooling treatment after exiting the furnace includes any one of argon, nitrogen or hydrogen, or a combination of at least two of them.

[0051] Preferably, the time for the cooling treatment after exiting the furnace is 5 to 30 minutes, for example: 5 minutes, 10 minutes, 15 minutes, 20 minutes or 30 minutes, etc.

[0052] Preferably, before the non-precious metal coating treatment on the cathode surface in step (3), the non-coated side of the substrate is glow cleaned.

[0053] Preferably, the bias voltage of the non-precious metal coating treatment on the cathode surface is 50-600V, for example, 50V, 100V, 200V, 300V or 600V, etc., preferably 100-400V.

[0054] Preferably, the current of the non-precious metal coating treatment on the cathode surface is 20-120A, for example: 20A, 50A, 80A, 100A or 120A, etc., preferably 40-100A.

[0055] Preferably, the gas used for the cathode surface non-precious metal coating treatment includes any one of Ar, N2, CH4, C2H2, TiCl4 or H2, or a combination of at least two of them.

[0056] Preferably, the gas flow rate of the cathode surface non-precious metal coating treatment is 100-500 sccm, for example: 100 sccm, 200 sccm, 300 sccm, 400 sccm or 500 sccm, etc., preferably 100-200 sccm.

[0057] Preferably, the cathode surface non-precious metal coating treatment time is 1 to 60 minutes, for example: 1 min, 5 min, 10 min, 30 min or 60 min, etc., preferably 5 to 30 minutes.

[0058] In a third aspect, the present invention provides a PEM electrolyzer, wherein the PEM electrolyzer comprises the PEM electrolyzer plate as described in the first aspect.

[0059] Compared with the prior art, the present invention has the following beneficial effects:

[0060] (1) The PEM electrolyzer electrode plate of the present invention uses precious metal + non-precious metal on the anode surface and non-precious metal coating on the cathode surface, which greatly reduces the use of precious metals. Adding a non-precious metal coating between the precious metal coating and the substrate can also further reduce the use of precious metal materials. Under the premise of excellent conductive performance, the bonding force is stronger and the corrosion resistance is higher.

[0061] (2) The method of the present invention makes it easier to control the thickness and thickness uniformity of the film layer, thereby ensuring the consistency of product quality, avoiding the waste liquid problem caused by electroplating or brushing in the industry, reducing the use of toxic organic solvents, and avoiding pollution to the environment.

[0062] (3) The contact resistance of the PEM electrolyzer plate of the present invention can reach 2.3 mΩ·cm at a pressure of 1.5 MPa. 2 Below, the corrosion current density can reach 0.84μA / cm 2 Below, by adjusting the plate material and preparation parameters, the contact resistance can reach 1.6 mΩ·cm 2, the corrosion current density can reach 0.61μA / cm 2 The performance is basically the same as that of plates plated with precious metals on both sides, but the cost is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 It is a schematic diagram of the structure of a PEM electrolytic cell plate made according to an embodiment of the present invention, wherein 101 is a metal plate substrate, 102 is anode surface non-precious metal coating, 103 is a precious metal coating, 104 is a first cathode surface non-precious metal coating, and 105 is a second cathode surface non-precious metal coating.

[0064] Figure 2 It is a schematic diagram of a pretreatment device according to an embodiment of the present invention, wherein 201 is a degreasing tank, 202 is a first water washing tank, 203 is a second water washing tank, 204 is a third water washing tank, and 205 is a drying box.

[0065] Figure 3 It is a schematic diagram of a coating device according to an embodiment of the present invention, wherein 301 is a pre-vacuum chamber, 302 is an ion cleaning chamber, 303 is a non-precious metal coating chamber, 304 is a precious metal coating chamber, and 305 is a coating cooling chamber. DETAILED DESCRIPTION

[0066] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0067] Example 1

[0068] This embodiment provides a PEM electrolyzer plate. During the preparation of the PEM electrolyzer plate, a schematic diagram of a pretreatment device is shown in FIG. Figure 2 The schematic diagram of the coating device is shown in Figure 3 As shown, the PEM electrolyzer plate is prepared by the following method:

[0069] (1) Select 316L stainless steel as the substrate. Place the substrate Figure 2The temperature shown is 60°C in the degreasing tank 201 containing 0.1% degreasing agent, and ultrasonic cleaning is performed for 5 minutes. After degreasing, the PEM electrolytic cell plates are immediately transferred to the pure water tanks 202, 203, and 204 in turn for cleaning for 2 minutes each, and finally the plates are dried at 80°C in the drying box 205 for 10 minutes. The pretreated PEM electrolytic cell plates are placed on the material rack of the PVD furnace, and the cathode surfaces of the two plates are attached together. They are placed in the pre-vacuum chamber 301 and the furnace door is closed for pre-vacuuming. After reaching the background vacuum, they are transferred to the ion cleaning chamber 302 for ion cleaning. During the cleaning process, 200sccm of Ar gas is introduced at a pressure of 5Pa, and glow cleaning is performed under a bias of 1100V. During the cleaning process, the Hall ion source is turned on, the power of the ion source is 2.2KW, the energy of the ion beam is selected to be 300eV, and the cleaning time is 20min;

[0070] (2) The substrate is transferred to the non-precious metal coating chamber 303, and a Ti target is used for coating. During the coating process, 150 sccm of nitrogen is introduced, the bias voltage is selected to be 350 V, and the current is 90 A. The coating time is 20 minutes to form a layer of TiN coating. Transfer to the precious metal coating chamber 304, and a precious metal Pt target is used for coating. The coating is carried out with 100 sccm of argon gas, the bias voltage is selected to be 300 V, the coating time is 5 minutes, and the coating temperature is selected to be 200°C. The electrode plate is transferred to the coating cooling chamber 305 for cooling. During the cooling process, 100 sccm of nitrogen is introduced for cooling. The cooling time is 5 minutes;

[0071] (3) Remove the plated electrode, reverse the front and back surfaces of the two plates, and bond the anode surfaces coated with precious metals together. Place the rack into the pre-vacuum chamber 301 and close the furnace door to evacuate the chamber to a base vacuum of 1×10 -3 After Pa, the ion cleaning chamber 302 is placed and 200 sccm of Ar gas is introduced to perform glow cleaning at a bias voltage of 1000V. During the cleaning process, the Hall ion source is turned on, the power of the ion source is 2.2KW, and the energy of the ion beam is selected to be 300eV. After cleaning, it is placed in the non-precious metal coating chamber 303, and a Ti target is used for coating. During the coating process, 300sccm of nitrogen is added, the bias voltage is selected to be 350V, the current is 60A, and the coating time is 30min to form a layer of TiN coating. Then, it is transferred to the precious metal coating chamber 304 and a graphite target is used for coating (here, the graphite coating can be completed in the precious metal coating chamber in order to save equipment). The coating is carried out with 200sccm of argon, the bias voltage is selected to be 300V, the current is 40A, the coating time is 10min, and the coating temperature is selected to be 260°C. The plate is transferred to the coating cooling chamber 305 for cooling, during which 100sccm of nitrogen is introduced for cooling, and the cooling time is 5min to obtain the PEM electrolytic cell plate.

[0072] The structural schematic diagram of the PEM electrolyzer plate is as follows Figure 1 As shown, it includes a metal plate substrate 101, an anode surface non-precious metal layer 102 with a thickness of 400nm, a precious metal layer 103 with a thickness of 80nm, a first cathode surface non-precious metal layer 104 with a thickness of 600nm and a second cathode surface non-precious metal layer 105 with a thickness of 200nm.

[0073] Example 2

[0074] This embodiment provides a PEM electrolyzer plate. During the preparation of the PEM electrolyzer plate, a schematic diagram of a pretreatment device is shown in FIG. Figure 2 The schematic diagram of the coating device is shown in Figure 3 As shown, the PEM electrolyzer plate is prepared by the following method:

[0075] (1) Select 316L stainless steel as the substrate. Place the substrate Figure 2 The temperature shown is 40°C in the degreasing tank 201 containing 0.1% degreasing agent, and ultrasonic cleaning is performed for 5 minutes. After degreasing, the PEM electrolytic cell plates are immediately transferred to the pure water tanks 202, 203, and 204 in turn for cleaning for 2 minutes each, and finally the plates are dried at 60°C in the drying box 205 for 60 minutes. The pretreated PEM electrolytic cell plates are placed on the material rack of the PVD furnace, and the cathode surfaces of the two plates are attached together. Pre-vacuuming is performed in the pre-vacuum chamber 301. After reaching the background vacuum, they are transferred to the ion cleaning chamber 302 for ion cleaning. During the cleaning process, 100sccm of Ar gas is introduced with a pressure of 1Pa, and glow cleaning is performed under a bias of 500V. During the cleaning process, the Hall ion source is turned on, the power of the ion source is 2KW, the energy of the ion beam is selected to be 100eV, and the cleaning time is 40min;

[0076] (2) The substrate is transferred to the non-precious metal coating chamber 303, and a Cr target is used for coating. During the coating process, 150 sccm of nitrogen is introduced, the bias voltage is selected to be 100 V, and the current is 80 A. The coating time is 20 minutes to form a layer of CrN coating. Transfer to the precious metal coating chamber 304, and a precious metal Au target is used for coating. The coating is carried out with 150 sccm of argon gas, the bias voltage is selected to be 100 V, the coating time is 2 minutes, and the coating temperature is selected to be 200°C. The electrode plate is transferred to the coating cooling chamber 305 for cooling. During the cooling process, 100 sccm of nitrogen is introduced for cooling. The cooling time is 10 minutes;

[0077] (3) Remove the plated electrode, reverse the front and back sides of the two electrode plates, and bond the anode surfaces coated with precious metals together. Place the rack into the pre-vacuum chamber 301 of the furnace and close the furnace door to evacuate the vacuum until the background vacuum reaches 1×10 -3After Pa, the ion cleaning chamber 302 is placed and 200 sccm of Ar gas is introduced to perform glow cleaning at a bias voltage of 1000 V. During the cleaning process, the Hall ion source is turned on, the power of the ion source is 2.2KW, and the energy of the ion beam is selected to be 300eV. After cleaning, it is placed in the non-precious metal coating chamber 303, and a Cr target material is used for coating. During the coating process, 150sccm of nitrogen is added, the bias voltage is selected to be 350V, the current is 60A, and the coating time is 30min to form a layer of CrN coating. Then, it is transferred to the precious metal coating chamber 304 and a graphite target material is used for coating (here, the graphite coating can be completed in the precious metal coating chamber in order to save equipment). The coating is carried out with 200sccm of argon, the bias voltage is selected to be 300V, the current is 60A, the coating time is 20min, and the coating temperature is selected to be 260°C. The plate is transferred to the coating cooling chamber 305 for cooling, during which 100sccm of nitrogen is introduced for cooling, and the cooling time is 5min to obtain the PEM electrolytic cell plate.

[0078] The non-noble metal layer thickness of the anode surface of the PEM electrolyzer plate is 400nm, the noble metal layer thickness is 40nm, the non-noble metal layer thickness of the first cathode surface is 600nm, and the non-noble metal layer thickness of the second cathode surface is 400nm.

[0079] The structural schematic diagram of the PEM electrolyzer plate is as follows Figure 1 As shown, it includes a metal plate substrate 101, an anode surface non-precious metal layer 102 with a thickness of 400nm, a precious metal layer 103 with a thickness of 40nm, a first cathode surface non-precious metal layer 104 with a thickness of 600nm and a second cathode surface non-precious metal layer 105 with a thickness of 400nm.

[0080] Example 3

[0081] This embodiment provides a PEM electrolyzer plate. During the preparation of the PEM electrolyzer plate, a schematic diagram of a pretreatment device is shown in FIG. Figure 2 The schematic diagram of the coating device is shown in Figure 3 As shown, the PEM electrolyzer plate is prepared by the following method:

[0082] (1) Select 316L stainless steel as the substrate. Place the substrate Figure 2The temperature shown is 90°C in the degreasing tank 201 containing 0.1% degreasing agent, and ultrasonic cleaning is performed for 5 minutes. Immediately after degreasing, the PEM electrolytic cell plates are transferred to the pure water tanks 202, 203, and 204 in turn for cleaning for 2 minutes each, and finally the plates are dried at 160°C in the drying box 205 for 5 minutes. The pretreated PEM electrolytic cell plates are placed on the material rack of the PVD furnace, and the cathode surfaces of the two plates are attached together. They are placed in the pre-vacuum chamber 301 and the furnace door is closed for pre-vacuuming. After reaching the background vacuum, they are transferred to the ion cleaning chamber 302 for ion cleaning. During the cleaning process, 100sccm of Ar gas is introduced at a pressure of 10Pa, and glow cleaning is performed under a bias of 1500V. During the cleaning process, the Hall ion source is turned on, the power of the ion source is 3KW, the energy of the ion beam is selected to be 500eV, and the cleaning time is 50min;

[0083] (2) The substrate is transferred to the non-precious metal coating chamber 303 and coated by PECVD process. The substrate temperature is 300°C, the reaction gases are N2, CH4 and TiCl4, the total gas flow rate is 300sccm, the gas pressure is 5.0Pa, the pulse bias is 1500V, the frequency is 1200Hz, the duty cycle is 50%, and the coating time is 10min. Transfer to the precious metal coating chamber 304 and use the precious metal Pt target for coating. The coating uses 150sccm of argon gas, the bias voltage is selected to be 300V, the coating time is 10min, and the coating temperature is selected to be 200°C. The electrode plate is transferred to the furnace chamber 305 for cooling. During the cooling, 100sccm of nitrogen gas is introduced for cooling. The cooling time is 10min.

[0084] (3) Remove the plated electrode, reverse the front and back surfaces of the two plates, and bond the anode surfaces coated with precious metals together. Place the rack into the pre-vacuum chamber 301 and close the furnace door to evacuate the chamber to a base vacuum of 1×10 -3After Pa, it is placed in the ion cleaning chamber 302 and 200sccm of Ar gas is introduced, and glow cleaning is performed under a bias voltage of 1000V. During the cleaning process, the Hall ion source is turned on, the power of the ion source is 2.2KW, and the energy of the ion beam is selected to be 300eV. After cleaning, it is placed in the non-precious metal coating chamber 303 and coated by PECVD process. The substrate temperature is 300℃, the reaction gas is N2, CH4 and TiCl4, the total gas flow rate is 300sccm, the gas pressure is 5.0Pa, the pulse bias is 1500V, the frequency is 1200Hz, the duty cycle is 50%, and the coating time is 30min. Transfer to the precious metal coating chamber 304, use C target material for coating (here C coating can be completed in the precious metal coating chamber in order to save equipment), use 200sccm of argon gas for coating, the bias voltage is selected as 300V, the current is 60A, the coating time is 30min, the coating temperature is selected as 160°C, and the electrode plate is transferred to the coating cooling chamber 305 for cooling, during which 100sccm of nitrogen is introduced for cooling, and the cooling time is 5min to obtain the PEM electrolytic cell electrode plate.

[0085] The thickness of the non-precious metal layer on the anode side of the PEM electrolyzer plate is 150nm, the thickness of the precious metal layer is 160nm, the thickness of the non-precious metal layer on the first cathode side is 450nm, and the thickness of the non-precious metal layer on the second cathode side is 600nm.

[0086] The structural schematic diagram of the PEM electrolyzer plate is as follows Figure 1 As shown, it includes a metal plate substrate 101, an anode surface non-precious metal layer 102 with a thickness of 150nm, a precious metal layer 103 with a thickness of 160nm, a first cathode surface non-precious metal layer 104 with a thickness of 450nm and a second cathode surface non-precious metal layer 105 with a thickness of 600nm.

[0087] Example 4

[0088] This embodiment provides a PEM electrolyzer plate. During the preparation of the PEM electrolyzer plate, a schematic diagram of a pretreatment device is shown in FIG. Figure 2 As shown, 201 is a degreasing tank, 202 is a washing tank 1, 203 is a washing tank 2, 204 is a washing tank 3, 105 is a drying box, and the schematic diagram of the coating device is as shown in Figure 3 As shown, 301 is a pre-vacuum chamber 1, 302 is an ion cleaning chamber, 303 is a non-precious metal coating chamber, 304 is a precious metal coating chamber, and 305 is a coating cooling chamber. The PEM electrolytic cell plate is prepared by the following method:

[0089] (1) Select TA1 as the substrate. Place the substrate Figure 2The temperature shown is 60°C in the degreasing tank 201 containing 0.1% degreasing agent, and ultrasonic cleaning is performed for 5 minutes. After degreasing, the PEM electrolytic cell plates are immediately transferred to the pure water tanks 202, 203, and 204 in turn for cleaning for 2 minutes each, and finally the plates are dried at 80°C in the drying box 205 for 10 minutes. The pretreated PEM electrolytic cell plates are placed on the material rack of the PVD furnace, and the cathode surfaces of the two plates are attached together. They are placed in the pre-vacuum chamber 301 and the furnace door is closed for pre-vacuuming. After reaching the background vacuum, they are transferred to the ion cleaning chamber 302 for ion cleaning. During the cleaning process, 200sccm of Ar gas is introduced at a pressure of 5Pa, and glow cleaning is performed under a bias of 1100V. During the cleaning process, the Hall ion source is turned on, the power of the ion source is 2.2KW, the energy of the ion beam is selected to be 300eV, and the cleaning time is 20min;

[0090] (2) The substrate is transferred to the non-precious metal coating chamber 303 and coated by PECVD process. The substrate temperature is 300°C, the reaction gases are N2, CH4 and TiCl4, the total gas flow rate is 600sccm, the gas pressure is 5.0Pa, the pulse bias is 1500V, the frequency is 1200Hz, the duty cycle is 50%, and the coating time is 30min. Transfer to the precious metal coating chamber 304 and use the precious metal Pt target for coating. The coating uses 100sccm of argon gas, the bias voltage is selected to be 300V, the coating time is 5min, and the coating temperature is selected to be 200°C. The electrode plate is transferred to the furnace chamber 305 for cooling. During the cooling, 100sccm of nitrogen gas is introduced for cooling. The cooling time is 5min.

[0091] (3) Remove the plated electrode, reverse the front and back surfaces of the two plates, and bond the anode surfaces coated with precious metals together. Place the rack into the pre-vacuum chamber 301 and close the furnace door to evacuate the chamber to a base vacuum of 1×10 -3After 1000V, the substrate was placed in the ion cleaning chamber 302, and 200sccm of Ar gas was introduced. The glow cleaning was performed under a bias voltage of 1000V. During the cleaning process, the Hall ion source was turned on. The power of the ion source was 2.2KW, and the energy of the ion beam was selected to be 300eV. After cleaning, the substrate was placed in the non-precious metal coating chamber 303 and the PECVD process was used for coating. The substrate temperature was 300℃, the reaction gases were N2, CH4 and TiCl4, the total gas flow rate was 600sccm, the gas pressure was 5.0Pa, the pulse bias was 1500V, and the frequency was 1200. Hz, the duty cycle is 50%, the coating time is 30min, and it is transferred to the precious metal coating chamber 304, and C target material is used for coating (here, C coating can be completed in the precious metal coating chamber in order to save equipment), 200sccm of argon is used for coating, the bias voltage is selected as 300V, the current is 40A, the coating time is 10min, and the coating temperature is selected as 260℃. The plate is transferred to the cooling chamber 305 for cooling, during which 100sccm of nitrogen is introduced for cooling, and the cooling time is 5min to obtain the PEM electrolytic cell plate.

[0092] The thickness of the non-precious metal layer on the anode side of the PEM electrolyzer plate is 450nm, the thickness of the precious metal layer is 80nm, the thickness of the non-precious metal layer on the first cathode side is 450nm, and the thickness of the non-precious metal layer on the second cathode side is 200nm.

[0093] The structural schematic diagram of the PEM electrolyzer plate is as follows Figure 1 As shown, it includes a metal plate substrate 101, an anode surface non-precious metal layer 102 with a thickness of 450nm, a precious metal layer 103 with a thickness of 80nm, a first cathode surface non-precious metal layer 104 with a thickness of 450nm and a second cathode surface non-precious metal layer 105 with a thickness of 200nm.

[0094] Example 5

[0095] The difference between this embodiment and embodiment 1 is that the bias voltage of the non-precious metal coating treatment on the anode surface is 50V, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0096] Example 6

[0097] The only difference between this embodiment and embodiment 1 is that the bias voltage of the non-precious metal coating treatment on the anode surface is 600V, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0098] Example 7

[0099] The only difference between this embodiment and embodiment 1 is that the bias voltage of the noble metal coating process is 50V, and the other conditions and parameters are exactly the same as those of embodiment 1.

[0100] Example 8

[0101] The only difference between this embodiment and embodiment 1 is that the bias voltage of the noble metal coating process is 600V, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0102] Comparative Example 1

[0103] The only difference between this comparative example and Example 1 is that both sides of the electrode plate are the same non-precious metal layer + precious metal layer structure, and other conditions and parameters are exactly the same as those in Example 1.

[0104] Comparative Example 2

[0105] The only difference between this comparative example and Example 1 is that a conventional electroplating method is used to electroplate a precious metal layer on both sides of the electrode plate with a thickness of 200 nm. Other conditions and parameters are exactly the same as those in Example 1.

[0106] Performance Testing:

[0107] The plates prepared in the embodiments and comparative examples were subjected to contact resistance test and corrosion current density test. The contact resistance test was conducted under a pressure of 1.5 MPa, with at least 3 test points and the average value taken. The corrosion current density test was conducted by testing the anode surface of the plate containing the precious metal coating at a constant potential of 1.6 V for 1 h. The test results are shown in Table 1:

[0108] Table 1

[0109] <![CDATA[Contact resistance (mΩ·cm 2 )]]> <![CDATA[Corrosion current density (μA / cm 2 ).]]> Example 1 1.7 0.61 Example 2 2.3 0.74 Example 3 2.1 0.71 Example 4 1.6 0.66 Example 5 2.3 1.03 Example 6 2.2 1.15 Example 7 2.5 1.26 Example 8 2.5 1.17 Comparative Example 1 1.7 0.62 Comparative Example 2 2.9 1.56

[0110] As can be seen from Table 1, from Examples 1-4, the contact resistance of the PEM electrolyzer plate of the present invention can reach 2.3 mΩ·cm at a pressure of 1.5 MPa. 2 Below, the corrosion current density can reach 0.84μA / cm 2 Below, by adjusting the plate material and preparation parameters, the contact resistance can reach 1.6 mΩ·cm 2 , the corrosion current density can reach 0.61μA / cm 2 The performance is basically the same as that of plates plated with precious metals on both sides, but the cost is greatly reduced.

[0111] By comparing Example 1 with Examples 5-6, it can be seen that in the preparation process of the PEM electrolytic cell plate of the present invention, the bias voltage of the non-precious metal coating of the anode layer will affect its performance. The bias voltage of the non-precious metal coating of the anode layer is controlled at 100~400V, and the plate performance is better. If the bias voltage of the non-precious metal coating of the anode layer is too low, the bonding force of the non-precious metal layer is insufficient, and the conductivity and corrosion resistance are reduced; if the bias voltage of the non-precious metal coating of the anode layer is too high, the ion bombardment energy increases, the roughness of the coating increases, the corrosion area increases, and the corrosion resistance is reduced.

[0112] By comparing Example 1 with Examples 7-8, it can be seen that during the preparation process of the PEM electrolytic cell plate of the present invention, the bias voltage of the precious metal coating will affect its performance. When the bias voltage of the precious metal coating is controlled at 100-600V, the plate performance is better. If the bias voltage of the precious metal coating is too low, the deposition energy of the precious metal atoms during the coating process is low, the migration rate of the deposited atoms on the plate surface decreases, and a loose and porous microstructure is easily formed, which has an adverse effect on the corrosion resistance. If the bias voltage of the precious metal coating is too high, the back-sputtering ratio of the precious metal atoms increases, the material utilization rate decreases, and at the same time the surface roughness of the coating increases, the corrosion performance decreases, and the service life of the plate is shortened.

[0113] The contact resistance test and corrosion current density test of the plates obtained in Examples 1-4 and Comparative Examples 1-2 found that the performance of the PEM electrolytic cell plates of the present invention is consistent with that of the plates plated with Pt on both sides and the plates plated with Pt and C on both sides, but the amount of precious metal used is greatly reduced. The plates of the present invention are significantly improved in performance compared to traditional electroplated plates. Traditional electroplating is prone to defects such as pinholes, pits, and cracks, which have an adverse effect on the performance of the plates. The present application not only reduces the production cost, but also improves the structural stability of the plates.

[0114] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A PEM electrolyzer plate, characterized in that: The PEM electrolyzer plate includes a substrate and a cathode surface and an anode surface respectively arranged on the two side surfaces of the substrate, the anode surface includes a precious metal layer and an anode surface non-precious metal layer arranged between the substrate and the precious metal layer, and the cathode surface includes at least one cathode surface non-precious metal layer.

2. The PEM electrolyzer plate according to claim 1, characterized in that: The substrate includes any one of a stainless steel plate, a titanium plate, an aluminum plate, a copper plate or a nickel plate, or a combination of at least two of them.

3. The PEM electrolyzer plate according to claim 1, characterized in that: The noble metal layer includes any one of Au, Pt, Ta, Ru or Ir or a combination of at least two thereof; The anode surface non-noble metal layer includes a single substance layer and / or a compound layer; The single-substance layer includes any one of Ti, Nb, Cr, W or Ni, or a combination of at least two thereof; The compound layer includes any one of TiN, TiCN, TiC, NbC or CrN or a combination of at least two thereof; The thickness of the noble metal layer is 10-200 nm; The thickness of the non-noble metal layer on the anode surface is 100-800 nm.

4. The PEM electrolyzer plate according to claim 1, characterized in that: The cathode surface comprises a first cathode surface non-precious metal layer and a second cathode surface non-precious metal layer which are stacked in sequence; The first cathode side non-noble metal layer and the second cathode side non-noble metal layer independently include any one of a single substance layer, a compound layer, an amorphous carbon layer or a conductive polymer layer, or a combination of at least two thereof; The single-substance layer includes any one of Ti, Nb, Cr, W or C or a combination of at least two thereof; The compound layer includes any one of TiN, TiCN, TiC, NbC or CrN or a combination of at least two thereof; The thickness of the cathode surface non-noble metal layer is independently 100-800 nm.

5. A method for preparing a PEM electrolyzer plate according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) Glow cleaning of the substrate; (2) performing a non-precious metal coating treatment on the anode surface of the glow-cleaned substrate to obtain a non-precious metal layer on the anode surface, and performing a precious metal coating treatment on the surface of the non-precious metal layer on the anode surface to obtain a substrate provided with an anode surface; (3) On the other side of the substrate provided with the anode surface, a cathode surface non-precious metal coating treatment is performed to obtain the PEM electrolytic cell electrode plate.

6. The preparation method according to claim 5, characterized in that: The step (1) is performed before the glow cleaning. The pretreatment includes ultrasonic degreasing-ultrasonic pre-cleaning-secondary cleaning-pure water cleaning-drying; The temperature of the ultrasonic degreasing is 40-90°C; The drying temperature is 60-160°C; The glow cleaning includes cleaning the substrate in an inert atmosphere by means of negative glow discharge and an ion source; The bias voltage of the glow cleaning is 500~1500V; The pressure of the inert atmosphere is 0.5~80Pa; The ion source comprises any one of an anode layer ion source, a Hall ion source, a Kaufman ion source or a plasma source, or a combination of at least two thereof; The ion beam energy of the ion source is 100-500 eV; The power of the ion source is 2-3 kW; The glow cleaning time is 5 to 40 minutes.

7. The preparation method according to claim 5, characterized in that: The coating treatment device in step (2) includes a single converter and / or a continuous tunnel furnace; The coating treatment process includes any one of multi-arc ion plating, magnetron sputtering or evaporation plating or a combination of at least two thereof; The bias voltage of the non-precious metal coating treatment on the anode surface is 50-600V; The current for the non-precious metal coating treatment on the anode surface is 20-120A; The gas used for the non-precious metal coating treatment on the anode surface includes any one of Ar, N2, CH4, C2H2, TiCl4 or H2, or a combination of at least two thereof; The gas flow rate of the non-precious metal coating treatment on the anode surface is 100-500 sccm; The non-precious metal coating treatment time of the anode surface is 1 to 60 minutes.

8. The preparation method according to claim 5, characterized in that: The bias voltage of the precious metal coating treatment in step (2) is 100-600V; The gas flow rate of the noble metal coating process is 50-600 sccm; The precious metal coating treatment time is 2 to 20 minutes; After the noble metal coating treatment, a furnace cooling treatment is performed; The atmosphere for the cooling process after the furnace is taken out includes any one of argon, nitrogen or hydrogen, or a combination of at least two of them; The time for the cooling treatment after exiting the furnace is 5 to 30 minutes.

9. The preparation method according to claim 5, characterized in that: Step (3) glow cleaning the non-coated side of the substrate before the cathode surface is subjected to non-precious metal coating treatment; The bias voltage for non-precious metal coating treatment on the cathode side is 20~600V; The current for the non-precious metal coating treatment on the cathode surface is 20-120A; The gas used for the non-precious metal coating treatment on the cathode surface includes any one of Ar, N2, CH4, C2H2, TiCl4 or H2, or a combination of at least two thereof; The gas flow rate of the non-precious metal coating treatment on the cathode surface is 100-500 sccm; The cathode surface non-precious metal coating treatment time is 1 to 60 minutes.

10. A PEM electrolyzer, characterized in that: The PEM electrolyzer comprises the PEM electrolyzer plate according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Preparation method of PEM electrolytic cell anode bipolar plate

    CN114875464A

  • Preparation method of PEM electrolytic cell bipolar plate surface partition coating

    CN117026319A

  • Method of fabricating corrosion-resistant bipolar plate

    CN101095249A

  • Method for preparing protective coating on surface of bipolar plate of fuel cell

    CN108914060A

  • Preparation method and structure of anti-corrosion conductive coating and fuel cell pole plate

    CN112820890A