Method for preparing gradient alloy structure perovskite quantum dot nanofiber membrane based on microfluidic airflow spinning technology
The gradient alloy structure perovskite quantum dot nanofiber membrane was prepared through microfluidic control air flow spinning technology, which solved the problem of perovskite quantum dot stability and achieved efficient continuous production of perovskite quantum dot nanofiber membranes and high-quality Optical performance, suitable for display devices.
Patent Information
- Application Number
- CN202411310412.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-19
AI Technical Summary
The instability of perovskite quantum dots leads to poor stability in light, heat and air, affecting its service life in applications such as display devices. It is difficult for the existing technology to achieve continuous, scaled and stable Chemical production.
The microfluidic air flow spinning technology was used to prepare gradient alloy structure perovskite quantum dot nanofiber membranes. By introducing Rb+ doping and polyacrylonitrile coating, the in-situ of perovskite quantum dots is achieved by microfluidic air flow spinning method. Synthesis is made to form RbxCs1-xPbX3 perovskite quantum dot nanofiber membrane to enhance its stability.
This method significantly improves the stability of perovskite quantum dots and realizes large-scale continuous preparation. The prepared nanofiber membrane has high optical properties and is suitable for building high-color gamut backlight displays.
Smart Images

Figure CN119061582A_ABST
Abstract
Description
Technical Field
[0001] The present invention specifically relates to a preparation method for in-situ synthesizing perovskite quantum dots in polymer fibers under a controllable high-pressure airflow environment using nanofibers as reactors, and belongs to the technical field of preparation of novel nanomaterials and optoelectronic materials. Background Art
[0002] In recent years, the new generation of photoelectric conversion materials centered on perovskite quantum dots have attracted more and more attention and attention from domestic and foreign manufacturers and scientific researchers for their unique photoelectric properties, such as high quantum yield, coordinated emission and narrow half-peak width. They are expected to become the most promising materials in the fields of wide color gamut display, light-emitting diodes, sensors, solar cells and photocatalysts. Perovskite quantum dots (PQDs) mainly refer to a family of compounds with an ABX3 structure. The A position is usually a cation with a larger ionic radius (such as methylamine ions, cesium ions, etc.), and the B position is a metal cation with a smaller ionic radius (such as Pb 2+ , Sn 4+ Such materials have high luminous efficiency, and the emission wavelength can be precisely adjusted by controlling the composition and size. The tuning range can easily cover the entire visible light region, and the emission line is narrow (12nm to 40nm) with high color purity. The display device made of perovskite quantum dots has the characteristics of wide color gamut (~140%), even exceeding the commercialized OLED.
[0003] However, due to the inherent instability of perovskite quantum dots, such as the poor stability of the perovskite quantum dot ionic crystals to light, heat, moisture in the air, oxygen, etc., the service life of the device will be greatly reduced, which has become one of the urgent problems to be solved in this field. Up to now, it is still a huge challenge to achieve continuous, large-scale and stable production of perovskite quantum dots. Whether in the synthesis or use process, the crystal structure of perovskite quantum dots is prone to destruction, phase change, agglomeration, etc., resulting in significant fluorescence quenching, which puts forward extremely stringent conditions for the implementation plan of perovskite quantum dot preparation. Therefore, in order to improve the stability of perovskite quantum dots, researchers have proposed various methods and carried out a lot of fruitful preliminary work. The coating method is usually used to improve the stability of perovskite quantum dots. Polymers can encapsulate perovskite quantum dots in them. As a barrier to perovskite quantum dots, dense polymers can enhance the stability of water-sensitive materials, resist adverse external environments, and give them soft and easy-to-process properties. Summary of the invention
[0004] The present invention provides a method for preparing a gradient alloy structure perovskite quantum dot nanofiber membrane based on microfluidic airflow spinning technology, which solves the instability of the intrinsic structure of perovskite quantum dots in the prior art, discloses the Rb x Cs 1-x PbX3 perovskite quantum dots are selected and debugged to give them good practical application prospects.
[0005] The method for preparing a gradient alloy structure perovskite quantum dot nanofiber membrane based on microfluidic airflow spinning technology described in the present invention comprises the following specific steps:
[0006] Step 1: Measure a certain amount of organic solvent into a glass beaker;
[0007] Step 2: Weigh different proportions of rubidium halide (RbX), cesium halide (CsX) and lead halide (PbX2) into the beaker of step 1, and stir them magnetically until they are completely dissolved to obtain a clear and transparent solution;
[0008] Step 3: add an appropriate amount of organic ligand to the solution in step 2 and stir until uniform;
[0009] Step 4: Weigh 1.5 g of polyacrylonitrile (PAN) into the solution in step 3, and stir it magnetically at room temperature for 6 to 8 hours to completely dissolve it, thereby obtaining a transparent and uniform precursor spinning solution;
[0010] Step 5: Using the solution in step 4 as the spinning solution, a series of gradient alloy structured perovskite quantum dot nanofiber membranes are synthesized by a microfluidic airflow spinning machine.
[0011] Further, the organic solvent in step 1 is one of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) or a mixture thereof, the amount of DMF added is 7-10 mL, and the amount of DMSO added is 0-3 mL;
[0012] Further, the molar amount of RbX and CsX in step 2 is 0.13-0.39 mmol, the molar amount of PbX2 is 0.26-0.52 mmol, and the molar ratio of monovalent cation to lead precursor is controlled to be 1:1 in the entire precursor ratio;
[0013] Further, in the RbX, CsX, and PbX2 described in step 2, X is I and Br, that is, different molar amounts of RbI, CsI, RbBr, CsBr, PbI2, and PbBr2 are weighed respectively to synthesize Rb x Cs 1-x PbI3、RbxCs 1-x PbBr3, where x is 0.35 to 0.75;
[0014] Furthermore, the organic ligand in step 3 is selected as n-octylamine or oleylamine, and the amount of the ligand added is 0.05 to 0.30 mL;
[0015] Furthermore, in step 5, the air flow pressure of the microfluidic air-spinning machine is 0.4-0.8 MPa, and the flow rate of the syringe pump is 0.2-0.4 mL / min.
[0016] Rb obtained by the preparation method x Cs 1-x PbX3 perovskite quantum dot precursor spinning solution.
[0017] The Rb x Cs 1-x PbX3 perovskite quantum dot precursor spinning solution is used to prepare perovskite quantum dot nanofiber membrane based on microfluidic airflow spinning method.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] In the present invention, by introducing Rb + The preparation of A-site doped gradient alloy structure perovskite quantum dots was achieved by using polyacrylonitrile-coated Rb x Cs 1-x In situ synthesis of PbX3 perovskite quantum dot nanofiber membrane. The advantage of microfluidic airflow spinning method for preparing nanofiber membrane is that it can achieve large-scale continuous preparation. By designing a program to control the movement of the spinning needle, the uniform preparation of nanofiber membrane over a large area can be achieved, and the prepared nanofibers are collected on the nylon net of the collector to finally obtain the nanofiber membrane. During the spinning process, the volatilization of DMF is gradually controlled by airflow, effectively separating polyacrylonitrile and Rb x Cs 1-x Through the crystallization process of PbX3 quantum dots, nanofiber membranes with multiple colors of fluorescent emission were successfully prepared, with emission wavelengths ranging from 470 to 600nm.
[0020] In the present invention, Rb x Cs 1-x The PbX3 / PAN nanofiber membrane greatly improves the intrinsic stability of perovskite quantum dots. The batch-prepared perovskite quantum dots / polymer fibers form a nanofiber membrane with high optical properties, which can be used to construct a high color gamut backlight display. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Rb prepared in Example 1 0.5 Cs 0.5 Scanning electron microscopy diagram of PbI3 / PAN PQDs@red light nanofiber membrane;
[0022] Figure 2Rb prepared for Example 3 0.5 Cs 0.5 Scanning electron microscopy diagram of PbBr3 / PAN PQDs@green light nanofiber membrane;
[0023] Figure 3 Rb prepared for Example 5 0.5 Cs 0.5 Scanning electron microscopy diagram of PbBr3 / PAN PQDs@blue light nanofiber membrane;
[0024] Figure 4 Rb prepared in Example 1 0.5 Cs 0.5 Fluorescence spectrum of PbI3 / PAN PQDs@red light nanofiber membrane;
[0025] Figure 5 Rb prepared for Example 3 0.s Cs 0.5 Fluorescence spectrum of PbBr3 / PAN PQDs@green light nanofiber membrane;
[0026] Figure 6 Rb prepared for Example 5 0.5 Cs 0.5 Fluorescence spectrum of PbBr3 / PAN PQDs@blue light nanofiber membrane.
[0027] Specific implementation examples
[0028] The following is a clear and complete description of the technical solutions in the examples of the present invention. Obviously, the examples described are only part of the examples of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The following experimental methods and detection methods are conventional methods unless otherwise specified; the following reagents and raw materials are commercially available unless otherwise specified.
[0030] Example 1
[0031] Step 1: Measure 10 g of DMF into a glass beaker;
[0032] Step 2: Weigh 0.26 mmol RbI, 0.26 mmol CsI and 0.52 mmol PbI2 respectively into the beaker in step 1, and stir magnetically until they are completely dissolved to obtain a clear and transparent solution;
[0033] Step 3: Measure 0.19 mL of n-octylamine and add it to the solution in step 2 and stir until uniform;
[0034] Step 4: Weigh 1.5 g of polyacrylonitrile (PAN) into the solution in step 3, and stir it magnetically at room temperature for 6 to 8 hours to completely dissolve it, thereby obtaining a transparent and uniform precursor spinning solution;
[0035] Step 5: Using the solution in step 4 as the spinning solution, a series of gradient alloy structured perovskite quantum dot nanofiber membranes are synthesized by a microfluidic airflow spinning machine.
[0036] The Rb prepared in this example 0.5 Cs 0.5 The fluorescence emission peak of PbI3 / PAN PQDs nanofiber membrane is at 600.4nm, and its half-peak width is 29nm. 0.5 Cs 0.5 The PbI3 / PAN PQDs nanofiber membrane appears light yellow under sunlight and exhibits red fluorescence under 365nm ultraviolet light.
[0037] Example 2
[0038] Step 1: Measure 10 g of DMF into a glass beaker;
[0039] Step 2: Weigh 0.39 mmol RbI, 0.13 mmol CsI and 0.52 mmol PbI2 respectively into the beaker in step 1, and stir magnetically until they are completely dissolved to obtain a clear and transparent solution;
[0040] Step 3: Measure 0.19 mL of n-octylamine and add it to the solution in step 2 and stir until uniform;
[0041] Step 4: Weigh 1.5 g of polyacrylonitrile (PAN) into the solution in step 3, and stir it magnetically at room temperature for 6 to 8 hours to completely dissolve it, thereby obtaining a transparent and uniform precursor spinning solution;
[0042] Step 5: Using the solution in step 4 as the spinning solution, a series of gradient alloy structured perovskite quantum dot nanofiber membranes are synthesized by a microfluidic airflow spinning machine.
[0043] The Rb prepared in this example 0.75 Cs 0.25 The fluorescence emission peak position of PbI3 / PAN PQDs@red nanofiber membrane is 598nm, and its half-peak width is 28nm. 0.75 Cs 0.25 The PbI3 / PAN PQDs@red nanofiber membrane appears yellow under sunlight and exhibits red fluorescence under 365nm ultraviolet light.
[0044] Example 3
[0045] Step 1: Measure 10 g of DMF into a glass beaker;
[0046] Step 2: Weigh 0.26 mmol RbBr, 0.26 mmol CsBr and 0.52 mmol PbBr2 respectively into the beaker in step 1, and stir magnetically until they are completely dissolved to obtain a clear and transparent solution;
[0047] Step 3: Add 0.05 mL of oleylamine to the solution in step 2 and stir until uniform;
[0048] Step 4: Weigh 1.5 g of polyacrylonitrile (PAN) into the solution in step 3, and stir it magnetically at room temperature for 6 to 8 hours to completely dissolve it, thereby obtaining a transparent and uniform precursor spinning solution;
[0049] Step 5: Using the solution in step 4 as the spinning solution, a series of gradient alloy structured perovskite quantum dot nanofiber membranes are synthesized by a microfluidic airflow spinning machine.
[0050] The Rb prepared in this example 0.5 Cs 0.5 The fluorescence emission peak of PbBr3 / PAN PQDs@green nanofiber membrane is at 514nm, and its half-peak width is 25nm. 0.5 Cs 0.5 The PbBr3 / PAN PQDs@green nanofiber membrane appears yellow under sunlight and exhibits green fluorescence under 365nm ultraviolet light.
[0051] Example 4
[0052] Step 1: Measure 10 g of DMF into a glass beaker;
[0053] Step 2: Weigh 0.26 mmol RbBr, 0.26 mmol CsBr and 0.52 mmol PbBr2 respectively into the beaker in step 1, and stir magnetically until they are completely dissolved to obtain a clear and transparent solution;
[0054] Step 3: Add 0.27 mL of oleylamine to the solution in step 2 and stir until uniform;
[0055] Step 4: Weigh 1.5 g of polyacrylonitrile (PAN) into the solution in step 3, and stir it magnetically at room temperature for 6 to 8 hours to completely dissolve it, thereby obtaining a transparent and uniform precursor spinning solution;
[0056] Step 5: Using the solution in step 4 as the spinning solution, a series of gradient alloy structured perovskite quantum dot nanofiber membranes are synthesized by a microfluidic airflow spinning machine.
[0057] The Rb prepared in this example 0.5 Cs0.5 The fluorescence emission peak of PbBr3 / PAN PQDs@blue nanofiber membrane is at 475.9nm, and its half-peak width is 20nm. 0.5 Cs 0.5 The PbBr3 / PAN PQDs@blue nanofiber membrane appears light yellow under sunlight and exhibits blue fluorescence under 365nm ultraviolet light.
[0058] Example 5
[0059] Step 1: Measure 10 g of DMF into a glass beaker;
[0060] Step 2: Weigh 0.18 mmol RbBr, 0.34 mmol CsBr and 0.52 mmol PbBr2 respectively into the beaker in step 1, and stir magnetically until they are completely dissolved to obtain a clear and transparent solution;
[0061] Step 3: Add 0.14 mL of n-octylamine to the solution in step 2 and stir until uniform;
[0062] Step 4: Weigh 1.5 g of polyacrylonitrile (PAN) into the solution in step 3, and stir it magnetically at room temperature for 6 to 8 hours to completely dissolve it, thereby obtaining a transparent and uniform precursor spinning solution;
[0063] Step 5: Using the solution in step 4 as the spinning solution, a series of gradient alloy structured perovskite quantum dot nanofiber membranes are synthesized by a microfluidic airflow spinning machine.
[0064] The Rb prepared in this example 0.35 Cs 0.65 The fluorescence emission peak of PbBr3 / PAN PQDs@blue nanofiber membrane is at 473.6nm, with a half-peak width of 20nm. 0.35 Cs 0.65 The PbBr3 / PAN PQDs@blue nanofiber membrane appears light yellow under sunlight and exhibits blue fluorescence under 365nm ultraviolet light.
[0065] The samples in Example 1 were characterized and tested, and the results showed that:
[0066] See also Figure 1 , Figure 1 Rb prepared in Example 1 0.5 Cs 0.5 SEM image of PbI3 / PAN PQDs@red light nanofiber membrane sample. From the image, we can see that the diameter of nanofibers is evenly distributed, with an average diameter of about 500nm. The surface of nanofibers is smooth, indicating that during the spinning process, the polymer matrix solidifies rapidly and Rb is synthesized in situ. 0.5 Cs0.5 PbI3 quantum dots.
[0067] See also Figure 2 , Figure 2 Rb prepared in Example 3 0.5 Cs 0.5 The SEM image of the PbBr3 / PAN PQDs@green light nanofiber membrane sample shows that the diameter of the nanofibers is evenly distributed, with an average diameter of about 500nm. The surface of the nanofibers is smooth, indicating that during the spinning process, the polymer matrix solidifies rapidly and Rb is synthesized in situ. 0.5 Cs 0.5 PbBr3 quantum dots.
[0068] See also Figure 3 , Figure 3 Rb prepared in Example 4 0.5 Cs 0.5 The SEM image of the PbBr3 / PAN PQDs@Blue Light nanofiber membrane sample shows that the diameter of the nanofibers is evenly distributed, with an average diameter of about 500 nm. The surface of the nanofibers is smooth, indicating that during the spinning process, the polymer matrix solidifies rapidly and Rb is synthesized in situ. 0.5 Cs 0.5 PbBr3 quantum dots. See Figure 4 , Figure 4 Rb prepared in Example 1 0.5 Cs 0.5 The fluorescence spectrum of the PbI3 / PAN PQDs@red nanofiber membrane sample shows that the fluorescence emission peak is at 600.4nm and the half-peak width is 29nm. The inset is Rb 0.5 Cs 0.5 Photos of the PbI3 / PANPQDs@red nanofiber membrane taken under 365nm ultraviolet light and sunlight respectively show that the membrane appears light yellow under sunlight and exhibits red fluorescence under ultraviolet light.
[0069] See also Figure 5 , Figure 5 Rb prepared in Example 3 0.5 Cs 0.5 The fluorescence spectrum of the PbBr3 / PAN PQDs@green nanofiber membrane sample shows that the fluorescence emission peak is at 514nm and the half-peak width is 25nm. The inset is Rb 0.5 Cs 0.5 Photos of PbBr3 / PANPQDs@green nanofiber membrane taken under 365nm ultraviolet light and sunlight respectively show that the membrane appears yellow under sunlight and exhibits green fluorescence under ultraviolet light.
[0070] See also Figure 6 , Figure 6 Rb prepared in Example 4 0.5 Cs 0.5 The fluorescence spectrum of the PbBr3 / PAN PQDs@blue nanofiber membrane sample shows that the fluorescence emission peak is at 475.9nm and the half-peak width is 20nm. The inset is Rb 0.5 Cs 0.5 Photos of PbBr3 / PANPQDs@blue nanofiber membrane taken under 365nm ultraviolet light and sunlight respectively show that the membrane appears light yellow under sunlight and exhibits blue fluorescence under ultraviolet light.
[0071] The above results show that the Rb x Cs 1-x PbX3 / PAN PQDs nanofiber membrane achieves the regulation of the fluorescence color of perovskite quantum dots by adjusting the proportion of A-site cations in the precursor, the amount of ligand added, the type of halogen and the ratio between the halogens, and successfully invented the controllable preparation of red, green and blue light perovskite nanofiber membranes with gradient alloy structures.
[0072] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A method for preparing a gradient alloy structure perovskite quantum dot nanofiber membrane based on microfluidic airflow spinning technology, characterized in that: The following steps are involved: Step 1: Measure a certain amount of organic solvent into a glass beaker; Step 2: Weigh different proportions of rubidium halide (RbX), cesium halide (CsX) and lead halide (PbX2) into the beaker of step 1, and stir them magnetically until they are completely dissolved to obtain a clear and transparent solution; Step 3: add an appropriate amount of organic ligand to the solution in step 2 and stir until uniform; Step 4: Weigh 1.5 g of polyacrylonitrile (PAN) into the solution in step 3, and stir it magnetically at room temperature for 6 to 8 hours to completely dissolve it, thereby obtaining a transparent and uniform precursor spinning solution; Step 5: Using the solution in step 4 as the spinning solution, a series of gradient alloy structured perovskite quantum dot nanofiber membranes are synthesized by a microfluidic airflow spinning machine.
2. The preparation method according to claim 1, characterized in that The organic solvent in step 1 is one of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) or a mixture thereof, with the amount of DMF added being 7-10 mL and the amount of DMSO being 0-3 mL.
3. The preparation method according to claim 1, characterized in that The molar amount of RbX and CsX in step 2 is 0.13-0.39 mmol, the molar amount of PbX2 is 0.26-0.52 mmol, and the molar ratio of monovalent cation to lead precursor is controlled to be 1:1 in the entire precursor ratio.
4. The preparation method according to claim 1, characterized in that In step 2, X in RbX, CsX, and PbX2 is I and Br, that is, different molar amounts of RbI, CsI, RbBr, CsBr, PbI2, and PbBr2 are weighed respectively to synthesize Rb x Cs 1- x PbI3、Rb x Cs 1-x PbBr3, wherein x is 0.35 to 0.
75.
5. The preparation method according to claim 1, characterized in that The organic ligand in step 3 is selected as n-octylamine or oleylamine, and the amount of the ligand added is 0.05-0.30 mL.
6. The preparation method according to claim 1, characterized in that In step 5, the air flow pressure of the microfluidic air spinning machine is 0.4-0.8 MPa, and the flow rate of the injection pump is 0.2-0.4 mL / min.
Citation Information
Patent Citations
Method for passivating surface defects of all-inorganic perovskite quantum dots and application thereof
CN116904193A
Perovskite material for intelligent window, perovskite thermochromism method induced by polar solvent vapor and application of perovskite thermochromism method in intelligent device
CN118479530A
BIO-sensing nanodevice
WO2009018467A2
Cited By
Preparation method of lead-free double perovskite nanofiber capable of efficiently photocatalysis CO2 reduction
CN119777019A