Efficient antistatic agent for spandex wrap yarn oiling agent and preparation method of efficient antistatic agent
By using highly efficient antistatic agents of glycol, phosphate derivatives and modified graphene in spandex coated yarn oil agent, the problem of insufficient conductivity of existing antistatic agents is solved, and excellent antistatic properties are achieved. Good compatibility significantly improves the conductivity and use effect of the oil agent.
Patent Information
- Application Number
- CN202411528172.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-10-30
AI Technical Summary
The conductivity of existing antistatic agents in spandex coated yarn oil agents is insufficient, resulting in poor antistatic performance and cannot meet market demand.
Ethylene glycol, phosphate derivatives and modified graphene are used as high-efficiency antistatic agents to form stable antistatic agents through reasonable proportions, and are uniformly dispersed in spandex coated yarn oil agent through ultrasonic dispersion technology. Modified graphene has good compatibility with other components.
It significantly improves the conductivity of spandex coated yarn oil agent, effectively reduces static accumulation, improves anti-static properties, and has good compatibility with other components, can be evenly dispersed, significantly improving the use effect of the oil agent.
Smart Images

Figure SMS_6 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of antistatic agent technology, specifically relating to a high-efficiency antistatic agent for spandex-coated yarn oiling and its preparation method. Background Art
[0002] Spandex-covered yarn is an elastic yarn formed by covering elongated spandex filaments with long or short fiber yarns (such as polyester) in a spiral pattern, using spandex filaments as the core. As a high-performance textile material, spandex-covered yarn possesses excellent elasticity and resilience due to its core yarn being spandex, while the outer yarn enhances its strength, abrasion resistance, and high-temperature resistance. The covering process results in even yarn texture, a smooth surface, and good luster. With its high elasticity, abrasion resistance, high-temperature resistance, evenness, strength, and stability, spandex-covered yarn has been widely used and recognized in textiles across many fields, including clothing, medical, and sports.
[0003] Spandex-covered yarn oil is a specialized oil used in the production of spandex-covered yarn. It is primarily applied to the surface of the yarn to improve its lubricity, antistatic properties, bundling ability, and processability. During the production process, the oil also reduces friction between the yarn and equipment, preventing yarn breakage, improving production efficiency, and giving the yarn a good hand feel and appearance. The main components of spandex-covered yarn oil include mineral oil, silicone oil, antistatic agents, and emulsifiers. These components are mixed through specific formulations and processes to ensure that the oil meets the various performance requirements of spandex-covered yarn production. Antistatic agents, as an essential component of spandex-covered yarn oil, not only require excellent antistatic properties but also good compatibility with other components to improve the effectiveness of the oil.
[0004] Chinese patent application CN202310549066.5 discloses an antistatic agent for use in chemical fiber spinning oils and its preparation method. The antistatic agent comprises epoxy-modified silicone oil, hydroxyl-terminated polyether, and phosphorus pentoxide. The molar ratio of epoxy-modified silicone oil, hydroxyl-terminated polyether, and phosphorus pentoxide is 1:2-3:0.5-2. Phosphorus pentoxide reacts with the reaction products of epoxy-modified silicone oil and hydroxyl-terminated polyether to generate polyether silicone oil phosphate ester with antistatic properties. However, the conductivity of the polyether silicone oil phosphate ester mixed with methyl silicone oil is less than 0.500 mS·cm. -1 Its antistatic properties are insufficient; therefore, it is necessary to develop a high-efficiency antistatic agent suitable for spandex-coated yarn oil to meet market demand. Summary of the Invention
[0005] The purpose of this invention is to address the shortcomings of existing technologies by providing a high-efficiency antistatic agent for spandex-coated yarn oiling and its preparation method. The high-efficiency antistatic agent includes ethylene glycol, phosphate ester derivatives, and modified graphene, wherein ethylene glycol acts as a stabilizer. Through reasonable formulation, a stable antistatic agent can be formed. When used in spandex-coated yarn oiling, it exhibits excellent antistatic properties, can be uniformly dispersed in the spandex-coated yarn oiling, and has good compatibility with other components.
[0006] The technical solution adopted by the present invention to achieve the above objectives is as follows: A high-efficiency antistatic agent for use in spandex-coated yarn oiling, the high-efficiency antistatic agent comprising ethylene glycol, phosphate ester derivatives and modified graphene; the mass ratio of ethylene glycol, phosphate ester derivatives and modified graphene is 5:4-5:0.8-1; In the technical solution of this invention, the preparation method of the modified graphene is as follows: N,N-dimethylformamide and graphene oxide are added to a reaction vessel and mixed evenly. Phosphate ester derivative and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride are added, the temperature is raised to 55-60℃, and the reaction is stirred for 4-6 hours. After the reaction is completed, the mixture is cooled, filtered, and the filter residue is washed repeatedly with water and ethanol in sequence. After drying, modified graphene oxide is obtained.
[0007] Furthermore, the mass ratio of the graphene oxide, the phosphate derivative, and the 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride is 1:0.2-0.3:0.1-0.15.
[0008] In the technical solution of this invention, the preparation method of the phosphate ester derivative is as follows: S1. Add chloroform, p-nitrobenzyl alcohol, and triethylamine to the reaction vessel, mix thoroughly, and slowly add epichlorohydrin dropwise. After the addition is complete, raise the temperature to 55-60℃ and stir the reaction for 4-5 hours. After the reaction is complete, remove the chloroform, extract with water and dichloromethane, and concentrate the organic phase under reduced pressure to obtain p-nitrobenzyl alcohol. The chemical structural formula is: ; S2. Add chloroform, p-nitrobenzenealkyl alcohol, and concentrated sulfuric acid to the reaction vessel, mix thoroughly, heat to 55-60℃, and slowly add dimethyl phosphite dropwise. After the addition is complete, continue stirring the reaction for 3-4 hours. After the reaction is complete, remove chloroform, extract with water and dichloromethane, and concentrate the organic phase under reduced pressure to obtain p-nitrobenzene phosphate. The chemical structural formula is: ; S3. Add methanol, p-nitrophenyl phosphate, and palladium on carbon to the hydrogenation reactor, purge with 0.1 MPa hydrogen gas, and stir at room temperature for 6-7 hours. After the reaction is complete, filter off the palladium on carbon and wash with methanol. Concentrate the filtrate under reduced pressure to obtain p-aminophenyl phosphate, with the following chemical structural formula: ; S4. Add ethanol, p-aminophenyl phosphate, and dodecyl dimethyl tertiary amine to the reaction vessel, mix thoroughly, heat to 80℃, and reflux for 8-9 hours. After the reaction is complete, remove the ethanol, extract with water and dichloromethane, and concentrate the aqueous phase under reduced pressure to obtain the phosphate derivative. The chemical structural formula is: .
[0009] Furthermore, the molar ratio of p-nitrophenylethanol, epichlorohydrin, and triethylamine in step S1 is 1:1.0-1.1:1.3-1.5.
[0010] Furthermore, the molar ratio of p-nitrophenylalkyl alcohol, dimethyl phosphite, and concentrated sulfuric acid in step S2 is 1:1.1-1.2:0.1-0.2.
[0011] Furthermore, in step S3, the mass ratio of p-nitrophenyl phosphate to palladium on carbon is 1:0.1-0.15.
[0012] Further, the molar ratio of p-aminophenyl phosphate and dodecyl dimethyl tertiary amine in step S4 is 1:1.0-1.1.
[0013] The present invention also provides a method for preparing a high-efficiency antistatic agent for spandex-coated yarn oiling agents, comprising the following steps: adding ethylene glycol and phosphate derivatives to a reaction vessel according to the mass ratio, stirring evenly, adding modified graphene, and ultrasonically dispersing evenly to obtain a high-efficiency antistatic agent.
[0014] Furthermore, in the above-mentioned method for preparing a high-efficiency antistatic agent for spandex-coated yarn oil, the stirring speed is 500-600 r / min, the stirring time is 10-20 min, the ultrasonic power is 200-300 W, and the ultrasonic time is 0.5-1 h.
[0015] The present invention has the following beneficial effects: To obtain a high-efficiency antistatic agent for spandex-coated yarn oiling with better performance, this invention first uses p-nitrophenylethanol as a raw material, reacting it with epichlorohydrin and dimethyl phosphite to obtain p-nitrophenyl phosphate. After hydrogen reduction, it reacts with dodecyl dimethyl tertiary amine to prepare a phosphate derivative containing phenylamino, long-chain quaternary ammonium salt groups, and phosphate ester groups. The long-chain quaternary ammonium salt groups and phosphate ester groups endow the phosphate derivative with good dispersion stability and antistatic properties. Furthermore, this invention utilizes the phenylamino group in the phosphate derivative structure to react with the carboxyl group on the surface of graphene oxide, in a condensation process... Under the action of the compound 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, a condensation reaction occurs, thereby grafting phosphate ester derivative molecules onto the surface of graphene oxide to obtain modified graphene. The phosphate ester derivative molecules can endow graphene with good dispersion stability and antistatic properties. The modified graphene has good compatibility with other organic components. In this invention, the antistatic agent containing modified graphene is added to the oiling agent of spandex-coated yarn, which can greatly improve the conductivity of the oiling agent, more effectively conduct static electricity, reduce static electricity accumulation, and thus significantly improve its antistatic performance.
[0016] The high-efficiency antistatic agent provided by this invention includes ethylene glycol, phosphate ester derivatives and modified graphene, wherein ethylene glycol acts as a stabilizer. Through reasonable formulation, a stable antistatic agent can be formed. When used in spandex-coated yarn oiling agents, it has excellent antistatic properties, can be uniformly dispersed in spandex-coated yarn oiling agents, and has good compatibility with other components. Detailed Implementation
[0017] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the embodiments of the present application. Obviously, the described embodiments are only some embodiments of the present application, and not all embodiments. The technical features designed in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0018] In the technical solution of this invention, all chemical reagents used are commercially available. Graphene oxide was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; ethylene glycol CAS number 107-21-1; N,N-dimethylformamide CAS number 68-12-2; 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride CAS number 25952-53-8; p-nitrobenzeneethanol CAS number 100-27-6; triethylamine CAS number 121-44-8; epichlorohydrin CAS number 106-89-8; dimethyl phosphite CAS number 868-85-9; concentrated sulfuric acid CAS number 7664-93-9; dodecyl dimethyl tertiary amine CAS number 112-18-5; chloroform CAS number 67-66-3; ethanol CAS number 64-17-5; and methanol CAS number 67-56-1.
[0019] This embodiment provides a method for preparing a phosphate ester derivative, the synthetic route of which is as follows: ; S1. Add 600 mL of chloroform, 20.0 g of p-nitrobenzeneethanol, and 18.2 g of triethylamine to the reaction vessel, mix well, and slowly add 11.6 g of epichlorohydrin dropwise. After the addition is complete, raise the temperature to 60 °C and stir the reaction for 5 h. After the reaction is complete, remove the chloroform, extract with water and dichloromethane, and concentrate the organic phase under reduced pressure to obtain 25.8 g of p-nitrobenzenealkyl alcohol; wherein the molar ratio of p-nitrobenzeneethanol, epichlorohydrin, and triethylamine is 1:1.05:1.5. p-Nitrobenzenealkyl alcohol: ESI (m / z): 260.7 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 8.14 (d, J=8.5Hz, 2H), 7.52 (d, J=8.5Hz, 2H), 5.37 ( s, 1H), 4.11-4.15 (m, 1H), 3.64-3.70 (m, 4H), 3.38-3.42 (m, 2H), 2.85-2.89 (m, 2H); S2. Add 500 mL of chloroform, 25.0 g of p-nitrobenzenealkyl alcohol, and 1.9 g of concentrated sulfuric acid to the reaction vessel, mix well, heat to 60 °C, and slowly add 11.7 g of dimethyl phosphite dropwise. After the addition is complete, continue stirring for 4 h. After the reaction is complete, remove the chloroform, extract with water and dichloromethane, and concentrate the organic phase under reduced pressure to obtain 28.6 g of p-nitrobenzene phosphate; wherein the molar ratio of p-nitrobenzenealkyl alcohol, dimethyl phosphite, and concentrated sulfuric acid is 1:1.1:0.2. p-Nitrophenyl phosphate: ESI (m / z): 352.7 [M+H] + , 1H-NMR (600MHz, DMSO-d6, δppm): 8.15 (d, J=8.5Hz, 2H), 7.52 (d, J=8.5Hz, 2H), 4.01-4.06 (m, 1H), 3.64-3.70 (m, 10H), 3.41-3.46 (m, 2H), 2.86-2.91 (m, 2H); S3. Add 400 mL of methanol, 28.0 g of p-nitrophenyl phosphate and 2.8 g of palladium on carbon to the hydrogenation reactor, purge with 0.1 MPa hydrogen gas, and stir at room temperature for 7 h. After the reaction is complete, filter off the palladium on carbon and wash with methanol. Concentrate the filtrate under reduced pressure to obtain 22.2 g of p-aminophenyl phosphate; wherein the mass ratio of p-nitrophenyl phosphate to palladium on carbon is 1:0.1. p-Aminophenyl phosphate: ESI (m / z): 322.7 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 6.92 (d, J=8.4Hz, 2H), 6.45 (d, J=8.4Hz, 2H), 4.91 ( s, 2H), 4.01-4.05 (m, 1H), 3.66-3.72 (m, 10H), 3.42-3.45 (m, 2H), 2.73-2.76 (m, 2H); S4. Add 350 mL of ethanol, 22.0 g of p-aminophenyl phosphate, and 15.3 g of dodecyl dimethyl tertiary amine to the reaction vessel, mix well, heat to 80 °C, and reflux for 9 h. After the reaction is complete, remove the ethanol, extract with water and dichloromethane, and concentrate the aqueous phase under reduced pressure to obtain 30.5 g of phosphate derivative; wherein the molar ratio of p-aminophenyl phosphate to dodecyl dimethyl tertiary amine is 1:1.05. Phosphate ester derivative: ESI (m / z): 536.2 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 6.95 (d, J=8.4Hz, 2H), 6.43 (d, J=8.4Hz, 2H), 4.91 (s, 2H), 4.32-4.36 (m, 1H), 3.65-3.72 (m, 9H), 3.46-3.50 (m, 2H), 3.22-3.30 (m, 9H), 2.72-2.76 (m, 2H), 1.71-1.74 (m, 2H), 1.26-1.30 (m, 18H), 0.88 (t, J=6.9Hz, 3H).
[0020] A high-efficiency antistatic agent for use in the oiling of spandex-coated yarn, comprising ethylene glycol, a phosphate ester derivative, and modified graphene; the mass ratio of ethylene glycol, phosphate ester derivative, and modified graphene is 5:5:1. The modified graphene was prepared as follows: N,N-dimethylformamide and graphene oxide were added to a reaction vessel and mixed evenly. Then, a phosphate derivative and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride were added. The mixture was heated to 60°C and stirred for 5 hours. After the reaction was completed, the mixture was cooled, filtered, and the residue was washed repeatedly with water and ethanol. After drying, modified graphene oxide was obtained. The mass ratio of graphene oxide, phosphate derivative, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride was 1:0.3:0.15. The amount of N,N-dimethylformamide was 15 times the mass of graphene oxide.
[0021] A method for preparing a high-efficiency antistatic agent for spandex-coated yarn oiling includes the following steps: adding ethylene glycol and phosphate derivatives to a reaction vessel according to the mass ratio, stirring evenly, adding modified graphene, and ultrasonically dispersing evenly to obtain a high-efficiency antistatic agent; the stirring speed is 600 r / min, the stirring time is 15 min; the ultrasonic power is 200 W, and the ultrasonic time is 1 h.
[0022] A high-efficiency antistatic agent for use in the oiling of spandex-coated yarns, comprising ethylene glycol, phosphate ester derivatives, and modified graphene; the mass ratio of ethylene glycol, phosphate ester derivatives, and modified graphene is 5:4:0.9. The modified graphene was prepared as follows: N,N-dimethylformamide and graphene oxide were added to a reaction vessel and mixed evenly. Then, a phosphate derivative and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride were added. The mixture was heated to 55°C and stirred for 6 hours. After the reaction was completed, the mixture was cooled, filtered, and the residue was washed repeatedly with water and ethanol. After drying, modified graphene oxide was obtained. The mass ratio of graphene oxide, phosphate derivative, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride was 1:0.25:0.1. The amount of N,N-dimethylformamide was 15 times the mass of graphene oxide.
[0023] A method for preparing a high-efficiency antistatic agent for spandex-coated yarn oiling includes the following steps: adding ethylene glycol and phosphate derivatives to a reaction vessel according to the mass ratio, stirring evenly, adding modified graphene, and ultrasonically dispersing evenly to obtain a high-efficiency antistatic agent; the stirring speed is 550 r / min, the stirring time is 10 min; the ultrasonic power is 300 W, and the ultrasonic time is 0.5 h.
[0024] A high-efficiency antistatic agent for use in the oiling of spandex-coated yarns, comprising ethylene glycol, phosphate ester derivatives, and modified graphene; the mass ratio of ethylene glycol, phosphate ester derivatives, and modified graphene is 5:4.5:0.8. The modified graphene was prepared as follows: N,N-dimethylformamide and graphene oxide were added to a reaction vessel and mixed evenly. Then, a phosphate derivative and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride were added. The mixture was heated to 60°C and stirred for 4 hours. After the reaction was completed, the mixture was cooled, filtered, and the residue was washed repeatedly with water and ethanol. After drying, modified graphene oxide was obtained. The mass ratio of graphene oxide, phosphate derivative, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride was 1:0.2:0.13. The amount of N,N-dimethylformamide was 15 times the mass of graphene oxide.
[0025] A method for preparing a high-efficiency antistatic agent for spandex-coated yarn oiling includes the following steps: adding ethylene glycol and phosphate derivatives to a reaction vessel according to the mass ratio, stirring evenly, adding modified graphene, and ultrasonically dispersing evenly to obtain a high-efficiency antistatic agent; the stirring speed is 500 r / min, the stirring time is 20 min; the ultrasonic power is 250 W, and the ultrasonic time is 0.8 h.
[0026] A high-efficiency antistatic agent for use in the oiling of spandex-coated yarn, comprising ethylene glycol, a phosphate ester derivative, and modified graphene; the mass ratio of ethylene glycol, phosphate ester derivative, and modified graphene is 5:5:0.8. The modified graphene was prepared as follows: N,N-dimethylformamide and graphene oxide were added to a reaction vessel and mixed evenly. Then, a phosphate derivative and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride were added. The mixture was heated to 58°C and stirred for 5 hours. After the reaction was completed, the mixture was cooled, filtered, and the residue was washed repeatedly with water and ethanol. After drying, modified graphene oxide was obtained. The mass ratio of graphene oxide, phosphate derivative, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride was 1:0.3:0.1. The amount of N,N-dimethylformamide was 15 times the mass of graphene oxide.
[0027] A method for preparing a high-efficiency antistatic agent for spandex-coated yarn oiling includes the following steps: adding ethylene glycol and phosphate derivatives to a reaction vessel according to the mass ratio, stirring evenly, adding modified graphene, and ultrasonically dispersing evenly to obtain a high-efficiency antistatic agent; the stirring speed is 600 r / min, the stirring time is 20 min; the ultrasonic power is 300 W, and the ultrasonic time is 1 h.
[0028] Comparative Example 1 Compared with Example 2, the highly effective antistatic agent in this comparative example includes ethylene glycol, phosphate ester derivatives, and graphene oxide.
[0029] A high-efficiency antistatic agent for use in the oiling of spandex-coated yarn, comprising ethylene glycol, phosphate ester derivatives, and graphene oxide; the mass ratio of ethylene glycol, phosphate ester derivatives, and graphene oxide is 5:5:1. The preparation method of a high-efficiency antistatic agent for spandex-coated yarn oil is the same as that in Example 2.
[0030] Comparative Example 2 Compared with Example 2, the comparative example includes ethylene glycol, dodecyl phosphate salt and modified graphene as highly effective antistatic agents.
[0031] A high-efficiency antistatic agent for use in the oiling of spandex-coated yarns, comprising ethylene glycol, dodecyl phosphate salt, and modified graphene; the mass ratio of ethylene glycol, dodecyl phosphate salt, and modified graphene is 5:5:1. The preparation methods for modified graphene and a high-efficiency antistatic agent for spandex-coated yarn oil are the same as in Example 2.
[0032] Comparative Example 3 Compared with Example 2, the highly effective antistatic agent in this comparative example includes ethylene glycol, dodecyl phosphate salt, and graphene oxide.
[0033] A high-efficiency antistatic agent for use in the oiling of spandex-coated yarn, comprising ethylene glycol, dodecyl phosphate salt, and graphene oxide; the mass ratio of ethylene glycol, dodecyl phosphate salt, and graphene oxide is 5:5:1. The preparation method of a high-efficiency antistatic agent for spandex-coated yarn oil is the same as that in Example 2.
[0034] Performance testing 1.0g of the high-efficiency antistatic agent prepared in Examples 2-5 and Comparative Examples 1-3 was added to the spandex-coated yarn oil (15.0g glycerol monopalmitate, 5.0g propylene glycol random polyoxyethylene polyoxypropylene ether 1500, 2.0g propylene glycol fatty acid ester, 5.0g dimethyl silicone oil and 1.5g lauric acid polyoxyethylene ether) to test the conductivity of the spandex-coated yarn oil. The same amount of spandex-coated yarn oil was placed in a constant temperature water bath at 30℃ for 60 days to observe the stability of the oil. No stratification or precipitation was considered as stable. The spandex-coated yarn oil was also used in the spinning experiment of spandex-coated yarn to determine the static friction coefficient between yarns, the amount of static electricity on the yarn roll, and whether adhesion and yarn breakage occurred at an unwinding speed of 100m / min. The test results are shown in Table 1 below.
[0035] Table 1 Performance test results As shown in Table 1, the high-efficiency antistatic agent prepared in Examples 2-5 of this invention exhibits high conductivity when used in the oiling agent for spandex-coated yarn. During unwinding, there is no sticking or breakage, the static friction coefficient between yarns is low, and the amount of static electricity on the yarn roll is small, indicating excellent antistatic performance. Furthermore, the antistatic agent can be uniformly dispersed in the oiling agent for spandex-coated yarn with good stability, indicating good compatibility with other components. Compared with Comparative Examples 1-3, the phosphate ester derivative and modified graphene in the antistatic agent in Example 2 of this invention can jointly enhance the antistatic performance of the antistatic agent. In particular, the long-chain quaternary ammonium salt and phosphate ester groups grafted onto the surface of the modified graphene improve the dispersion stability of the modified graphene and its compatibility with other organic components, thereby greatly improving the conductivity of the oiling agent and more effectively discharging static electricity, reducing static accumulation.
[0036] It should be noted that, in this document, terms such as “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0037] Although the embodiments of the present application have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present application, and the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A high-efficiency antistatic agent for spandex coated yarn oil, characterized in that: The high-efficiency antistatic agent comprises ethylene glycol, phosphate derivatives and modified graphene; the mass ratio of the ethylene glycol, phosphate derivatives and modified graphene is 5:4-5:0.8-1; The preparation method of the modified graphene is as follows: adding N,N-dimethylformamide and graphene oxide into a reaction container, mixing them evenly, adding a phosphate derivative and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, heating to 55-60° C., stirring and reacting for 4-6 hours, cooling after the reaction is completed, filtering, and washing the filter residue repeatedly with water and ethanol in sequence, and drying to obtain the modified graphene oxide; The phosphate derivative is: 。 2. The high-efficiency antistatic agent for spandex coated yarn oil according to claim 1, characterized in that: The preparation method of the phosphate derivative is: S1. Add chloroform, p-nitrophenylethanol and triethylamine to a reaction vessel, mix well, slowly drop epichlorohydrin, raise the temperature to 55-60°C, stir and react for 4-5h, remove chloroform after the reaction is completed, extract with water and dichloromethane, and concentrate the organic phase under reduced pressure to obtain p-nitrophenyl alkyl alcohol; S2, add chloroform, p-nitrophenyl alkyl alcohol and concentrated sulfuric acid to the reaction container, mix well, heat to 55-60 ° C, slowly add dimethyl phosphite dropwise, continue to stir and react for 3-4 hours, after the reaction is completed, remove chloroform, use water and dichloromethane for extraction, and concentrate the organic phase under reduced pressure to obtain p-nitrophenyl phosphate; S3, add methanol, p-nitrophenyl phosphate and palladium carbon to the hydrogenation reaction kettle, pass 0.1 MPa hydrogen, stir and react at room temperature for 6-7 hours. After the reaction is completed, filter out the palladium carbon, wash with methanol, and concentrate the filtrate under reduced pressure to obtain p-aminophenyl phosphate; S4. Add ethanol, p-aminophenyl phosphate and dodecyl dimethyl tertiary amine to the reaction container, mix well, heat to 80°C, and reflux for 8-9 hours. After the reaction is completed, remove ethanol, extract with water and dichloromethane, and concentrate the aqueous phase under reduced pressure to obtain a phosphate derivative.
3. A high-efficiency antistatic agent for spandex coated yarn oil according to claim 2, characterized in that: The molar ratio of p-nitrophenylethanol, epichlorohydrin and triethylamine in step S1 is 1:1.0-1.1:1.3-1.
5.
4. A high-efficiency antistatic agent for spandex coated yarn oil according to claim 2, characterized in that: The molar ratio of p-nitrophenyl alkyl alcohol, dimethyl phosphite and concentrated sulfuric acid in step S2 is 1:1.1-1.2:0.1-0.
2.
5. The high-efficiency antistatic agent for spandex coated yarn oil according to claim 2, characterized in that: The mass ratio of p-nitrophenyl phosphate to palladium carbon in step S3 is 1:0.1-0.
15.
6. A high-efficiency antistatic agent for spandex coated yarn oil according to claim 2, characterized in that: The molar ratio of p-aminophenyl phosphate to dodecyl dimethyl tertiary amine in step S4 is 1:1.0-1.
1.
7. The high-efficiency antistatic agent for spandex coated yarn oil according to claim 1, characterized in that: In the preparation method of modified graphene, the mass ratio of graphene oxide, phosphate derivative and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride is 1:0.2-0.3:0.1-0.
15.
8. A method for preparing a high-efficiency antistatic agent for spandex coated yarn oil according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: adding ethylene glycol and phosphate derivatives into a reaction container according to a mass ratio, stirring evenly, adding modified graphene, and uniformly dispersing by ultrasonication to obtain a high-efficiency antistatic agent.
9. The method for preparing a high-efficiency antistatic agent for spandex coated yarn oil according to claim 8, characterized in that: The stirring speed is 500-600 r / min, and the stirring time is 10-20 min; the ultrasonic power is 200-300 W, and the ultrasonic time is 0.5-1 h.
Citation Information
Patent Citations
Siloxane modified graphene oxide, spandex spinning oil agent and preparation methods for siloxane modified graphene oxide and spandex spinning oil agent
CN111137881A
Dry antistatic spandex spinning oil and preparation method thereof
CN111206422A
Solvent-free bi-component spinning oil as well as preparation method and application thereof
CN115434044A
Elastic fiber prepared based on waste textiles and preparation method thereof
CN116516511A
MOF-fabric composites and methods of MOF-fabric composite synthesis
US20230149760A1