Preparation method of waterproof paint for paperboards

By applying waterproof coatings of desiccant, glue powder, polymer additives and borax on the cardboard, the water penetration problem caused by the damage of plastic film is solved, better waterproof effect is achieved, and the waterproof performance of cardboard is enhanced.

CN119061727APending Publication Date: 2024-12-03ZHONGHONG LANDSCAPE (HEBEI) NEW MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411356936.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the processing of cardboard, plastic film is only pasted on the surface of cardboard, which is prone to friction damage, causing water to penetrate into the cardboard, affecting the waterproofing effect.

Method used

A method of preparing cardboard waterproof coating is adopted. By mixing desiccant, glue powder, polymer additives, borax and tablet alkali in a specific proportion, it forms permeable waterproof coating, avoiding the use of plastic films, and the coating can form waterproof on the surface of cardboard. layer.

Benefits of technology

The waterproof thickness of the cardboard is enhanced, and waterproofing is prevented from penetrating into the cardboard through the damaged area, improving waterproof performance, and avoiding waterproof failure caused by the damage of plastic film.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a paperboard waterproof coating, and relates to the technical field of paperboard waterproofing. Comprising 6-8 kg of a drying agent, 11-13 kg of rubber powder, 3-6 kg of a polymer additive, 3-7 kg of borax, 0.5-2 kg of caustic soda flakes and 20-25 kg of water, the water is poured into a stirring barrel, the caustic soda flakes are added into the stirring barrel, the stirring time is 1-2 hours, and a prepared solution is obtained; adding rubber powder into the prepared solution, and fully stirring for 0.5-1 hour to obtain a gelatinized fluid; according to the waterproof coating disclosed by the invention, by arranging the rubber powder, the polymer additive, the borax and the caustic soda flakes, the waterproof coating is formed by matching, stirring and mixing the rubber powder, the polymer additive, the borax and the caustic soda flakes, so that the waterproof coating can permeate into a paperboard in the process of coating the paperboard with the waterproof coating, and the waterproof thickness of the waterproof coating is increased; and the situation that water can permeate into the paperboard through a damaged part when a plastic film is damaged due to friction is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of paperboard waterproofing, and in particular to a method for preparing a paperboard waterproof coating. Background Art

[0002] Cardboard, also known as board paper, is a thick paper sheet made of various pulps and composed of fibers interwoven with each other. The difference between cardboard and paper is usually distinguished by quantity and thickness. According to the purpose, it can be divided into packaging cardboard, such as boxboard, kraft boxboard, yellow cardboard, white cardboard, impregnated cushioning cardboard, etc.; industrial technical cardboard, such as electrical insulation cardboard, asphalt waterproof cardboard, etc.; building cardboard, such as felt paper, sound insulation cardboard, fireproof cardboard, gypsum cardboard, etc.; printing and decorative cardboard, such as font cardboard, cover cardboard, etc., the difference between board and paper, generally speaking, what we call paper, in a broad sense, includes the two terms paper and cardboard. In fact, the difference between paper and cardboard is only distinguished by its quantity. We usually call thin paper paper and thick paper cardboard.

[0003] In the process of cardboard processing, in order to improve the waterproof effect of cardboard when in use, a layer of plastic film is mostly coated on the surface of the cardboard. In actual use, the plastic film is only pasted on the surface of the cardboard, resulting in that when the plastic film is damaged by friction, water can penetrate into the cardboard through the damaged area. Therefore, a method for preparing a waterproof coating for cardboard is proposed. Summary of the invention

[0004] The purpose of the present invention is to solve the problem that a plastic film is only pasted on the surface of a cardboard, resulting in water being able to penetrate into the cardboard through the damaged part when the plastic film is damaged by friction. The present invention provides a method for preparing a waterproof coating for a cardboard.

[0005] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:

[0006] A method for preparing a paperboard waterproof coating comprises 6-8 kg of a desiccant, 11-13 kg of rubber powder, 3-6 kg of a polymer auxiliary agent, 3-7 kg of borax, 0.5-2 kg of caustic soda flakes and 20-25 kg of water.

[0007] Furthermore, the preparation method comprises:

[0008] S1: Pour water into a stirring barrel, and add caustic soda flakes into the stirring barrel, stirring for 1-2 hours to obtain a prepared solution;

[0009] S2: Adding the rubber powder into the prepared solution and stirring it thoroughly for 0.5-1 hour to obtain a gelatinized fluid;

[0010] S3: adding a polymer additive to the gelatinized fluid and stirring the fluid for 0.5-1 hour to obtain a modified fluid;

[0011] S4: adding borax to the modified fluid and stirring it for 0.5-1 hour to adjust the pH value of the modified fluid;

[0012] S5: Add desiccant to the modified fluid with adjusted pH, and stir for 0.5-1 hour to adjust the dryness of the modified fluid.

[0013] Furthermore, the mixing barrel can contain the materials and mix the materials at the same time.

[0014] Furthermore, the polymer auxiliary agent is a mixed solution of a leveling agent and a defoaming agent, with 1-2 kg of the leveling agent and 1.5-3 kg of the defoaming agent.

[0015] Furthermore, the rubber powder is processed and ground corn starch, and the corn starch particle size is 2-5 microns.

[0016] Furthermore, the borax particle distribution is D10, and the purity standard of borax refers to GB / T537-1997 "Industrial Disodium Tetraborate Decahydrate", in which the purity of borax should be 99.0% to 103.0%.

[0017] Furthermore, the purity standard of the caustic soda flakes refers to the primary standard of GB / T11199-2013 "High-purity Sodium Hydroxide", and the mass fraction of sodium hydroxide is ≧99.97%.

[0018] Furthermore, the alkalinity of the prepared solution is pH 9.5-11.

[0019] Furthermore, the pH value of the modified fluid is 6.8-7.2.

[0020] The beneficial effects of the present invention are as follows:

[0021] The present invention realizes the formation of waterproof coating by mixing and stirring the rubber powder, polymer additive, borax and caustic soda through the provision of rubber powder, polymer additive, borax and caustic soda. Therefore, in the process of coating the paperboard with the waterproof coating, the waterproof coating can penetrate into the inside of the paperboard, thereby increasing the waterproof thickness of the waterproof coating, avoiding the use of plastic film, resulting in water penetrating into the paperboard through the damaged part when the plastic film is damaged by friction. DETAILED DESCRIPTION

[0022] A method for preparing a paperboard waterproof coating comprises 8 kg of a desiccant, 1.25 kg of rubber powder, 4 kg of a polymer auxiliary agent, 5 kg of borax, 1 kg of caustic soda flakes and 22.5 kg of water.

[0023] The preparation method comprises:

[0024] S1: Pour water into a stirring barrel, and add caustic soda flakes into the stirring barrel, stirring for 2 hours to obtain a prepared solution;

[0025] S2: Adding rubber powder into the prepared solution and stirring thoroughly for 0.5 hours to obtain gelatinized fluid;

[0026] S3: adding a polymer additive to the gelatinized fluid and stirring the fluid for 0.5 hours to obtain a modified fluid;

[0027] S4: adding borax to the modified fluid and stirring it for 0.5 hours to adjust the pH value of the modified fluid;

[0028] S5: Add desiccant to the modified fluid with adjusted pH, and adjust the dryness of the modified fluid by stirring for 0.5 hours.

[0029] The mixing barrel can hold the materials and mix them at the same time.

[0030] The polymer additive is a mixed solution of a leveling agent and a defoaming agent, including 2 kg of leveling agent and 2 kg of defoaming agent. Specifically, the leveling agent helps to form a smooth coating surface to ensure that the coating has good fluidity and surface tension balance after coating. The defoaming agent is used to reduce the foam generated during the production and construction of the coating, thereby ensuring the use effect of the coating after coating.

[0031] The rubber powder is processed and ground corn starch, and the particle size of corn starch is 3 microns.

[0032] The particle distribution of borax is D10, and the purity standard of borax refers to GB / T537-1997 "Industrial Disodium Tetraborate Decahydrate", in which the purity of borax should be 99.9%.

[0033] The purity standard of caustic soda flakes refers to the first-level standard of GB / T11199-2013 "High-purity Sodium Hydroxide", and its mass fraction of sodium hydroxide is ≥99.97%.

[0034] The alkalinity of the prepared solution is PH10. Specifically, after the flake caustic soda is added to the water, the pH value of the water is adjusted to provide an alkaline environment, which helps to ensure sufficient gelatinization of the starch. Under alkaline conditions, the starch in the corn flour will gelatinize, that is, the starch granules absorb water, swell and dissolve. This gelatinization process can improve the processing characteristics of the corn flour and increase its plasticity and viscosity during processing.

[0035] The pH value of the modified fluid is PH7. Specifically, borax can be used as a cross-linking agent or a water-retaining agent and is added after the polymer additive. The addition of borax helps to improve the adhesion strength of the coating and improve the coating performance. The mixture of flake caustic soda and borax can undergo an acid-base neutralization reaction, thereby adjusting the pH value of the modified fluid and avoiding affecting the use of alkaline or acidic desiccants. The desiccant can be a silica gel desiccant, a montmorillonite desiccant or a calcium chloride desiccant, thereby controlling the moisture content of the waterproof coating.

[0036] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a paperboard waterproof coating, characterized in that: It includes 6-8 kg of desiccant, 11-13 kg of rubber powder, 3-6 kg of polymer additives, 3-7 kg of borax, 0.5-2 kg of flake caustic soda and 20-25 kg of water.

2. The method for preparing a paperboard waterproof coating according to claim 1, characterized in that: The preparation method comprises: S1: Pour water into a stirring barrel, and add caustic soda flakes into the stirring barrel, stirring for 1-2 hours to obtain a prepared solution; S2: Adding the rubber powder into the prepared solution and stirring it thoroughly for 0.5-1 hour to obtain a gelatinized fluid; S3: adding a polymer additive to the gelatinized fluid and stirring the fluid for 0.5-1 hour to obtain a modified fluid; S4: adding borax to the modified fluid and stirring it for 0.5-1 hour to adjust the pH value of the modified fluid; S5: Add desiccant to the modified fluid with adjusted pH, and stir for 0.5-1 hour to adjust the dryness of the modified fluid.

3. The method for preparing a paperboard waterproof coating according to claim 2, characterized in that: The mixing barrel can contain the materials and mix the materials at the same time.

4. The method for preparing a paperboard waterproof coating according to claim 2, characterized in that: The polymer auxiliary agent is a mixed solution of a leveling agent and a defoaming agent, with 1-2 kg of the leveling agent and 1.5-3 kg of the defoaming agent.

5. The method for preparing a paperboard waterproof coating according to claim 2, characterized in that: The rubber powder is processed and ground corn starch, and the corn starch particle size is 2-5 microns.

6. The method for preparing a paperboard waterproof coating according to claim 2, characterized in that: The particle distribution of the borax is D10, and the purity standard of borax refers to GB / T537-1997 "Industrial Disodium Tetraborate Decahydrate", in which the purity of borax should be 99.0% to 103.0%.

7. The method for preparing a paperboard waterproof coating according to claim 2, characterized in that: The purity standard of the caustic soda flakes refers to the first-level standard of GB / T11199-2013 "High-purity Sodium Hydroxide", and the mass fraction of sodium hydroxide is ≧99.97%.

8. The method for preparing a paperboard waterproof coating according to claim 2, characterized in that: The alkalinity of the prepared solution is pH 9.5-11.

9. The method for preparing a paperboard waterproof coating according to claim 2, characterized in that: The pH value of the modified fluid is 6.8-7.

2.

10. A paperboard waterproof coating obtained according to the method for preparing a paperboard waterproof coating according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • High-strength moisture-proof paperboard surface treatment agent

    CN102838945A

  • Glue for producing corrugated case at high speed and preparation method thereof

    CN103756591A

  • Coating glue and process for producing cartons

    CN109913147A

  • Environment-friendly one-step glue preparation method

    CN111205789A

  • Starch-mixed adhesive for manufacturing reinforced corrugated cores

    KR1019930013043A